Find suppliers for this alloyC10200
Chemical Composition
Element
Cu(1,2,3)O
(1) Cu is determined by the difference between the impurity total and 100%. (2) This is a high conductivity copper which has, in the annealed condition a minimum conductivity of 100% IACS except for Alloy C10100 which has a minimum conductivity of 101% IACS. (3) Cu value includes Ag.
Min (%)99.95
Max (%)0.0010
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell F scale
Rockwell 30T scale
Shear Strength
(ksi)
Fatigue Strength**
(ksi)
Section Size
(in)
Cold Work
(%)
Flat Products1/2 HardH0242   Typ
36   Typ
14   Typ
40   Typ
84   Typ
50   Typ
26   Typ
13   Typ
0.04
1/4 HardH0138   Typ
30   Typ
25   Typ
25   Typ
70   Typ
36   Typ
25   Typ
0.04
H0138   Typ
30   Typ
35   Typ
25   Typ
70   Typ
25   Typ
0.25
1/8 HardH0036   Typ
28   Typ
40   Typ
10   Typ
60   Typ
25   Typ
0.25
H0036   Typ
28   Typ
30   Typ
10   Typ
60   Typ
25   Typ
25   Typ
0.04
As Hot RolledM2034   Typ
10   Typ
45   Typ
45   Typ
23   Typ
0.04
M2032   Typ
10   Typ
50   Typ
40   Typ
22   Typ
0.25
Extra SpringH1057   Typ
53   Typ
4   Typ
62   Typ
95   Typ
64   Typ
29   Typ
0.04
HardH0450   Typ
45   Typ
12   Typ
50   Typ
90   Typ
28   Typ
0.25
H0450   Typ
45   Typ
6   Typ
50   Typ
90   Typ
57   Typ
28   Typ
13   Typ
0.04
H0445   Typ
40   Typ
20   Typ
45   Typ
85   Typ
26   Typ
1
Nominal Grain Size 0.025 mmOS02534   Typ
11   Typ
45   Typ
45   Typ
23   Typ
11   Typ
0.04
Nominal Grain Size 0.050 mmOS05032   Typ
10   Typ
45   Typ
40   Typ
22   Typ
0.04
OS05032   Typ
10   Typ
50   Typ
40   Typ
22   Typ
0.25
SpringH0855   Typ
50   Typ
4   Typ
60   Typ
94   Typ
63   Typ
29   Typ
14   Typ
0.04
RodAs Hot RolledM2032   Typ
10   Typ
55   Typ
40   Typ
22   Typ
1
HardH0455   Typ
50   Typ
10   Typ
60   Typ
94   Typ
29   Typ
0.2540
H0448   Typ
44   Typ
16   Typ
47   Typ
87   Typ
27   Typ
17   Typ
135
H0445   Typ
40   Typ
20   Typ
45   Typ
85   Typ
26   Typ
216
Nominal Grain Size 0.050 mmOS05032   Typ
10   Typ
55   Typ
40   Typ
22   Typ
1
ShapesAs Hot ExtrudedM3032   Typ
10   Typ
50   Typ
40   Typ
22   Typ
0.5
As Hot RolledM2032   Typ
10   Typ
50   Typ
40   Typ
22   Typ
0.5
HardH0440   Typ
32   Typ
30   Typ
35   Typ
26   Typ
0.515
Nominal Grain Size 0.050 mmOS05032   Typ
10   Typ
50   Typ
40   Typ
22   Typ
0.5
TubeHard DrawnH8055   Typ
50   Typ
8   Typ
60   Typ
95   Typ
63   Typ
29   Typ
0.06540
Light Drawn, Light Cold RolledH5540   Typ
32   Typ
25   Typ
35   Typ
77   Typ
45   Typ
26   Typ
0.06515
Nominal Grain Size 0.025 mmOS02534   Typ
11   Typ
45   Typ
45   Typ
23   Typ
0.065
Nominal Grain Size 0.050 mmOS05032   Typ
10   Typ
45   Typ
40   Typ
22   Typ
0.065
WireHardH0455   Typ
1.5   Typ
29   Typ
0.08
Nominal Grain Size 0.050 mmOS05035   Typ
35   Typ
24   Typ
0.08
SpringH0866   Typ
1.5   Typ
33   Typ
0.08
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
Melting Point - Liquidus°F1981
Melting Point - Solidus°F1981
Densitylb/cu in. at 68°F0.323
Specific Gravity8.94
Electrical Conductivity% IACS at 68°F101
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F226
Coefficient of Thermal Expansion 68-21210⁻⁶ per °F (68 – 212°F)9.4
Coefficient of Thermal Expansion 68-39210⁻⁶ per °F (68 – 392°F)9.6
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)9.8
Specific Heat CapacityBtu/ lb /°F at 68°F0.092
Modulus of Elasticity in Tensionksi17000
Modulus of Rigidityksi6400
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingFair
Gas Shielded Arc WeldingGood
Coated Metal Arc WeldingNot Recommended
Spot WeldNot Recommended
Seam WeldNot Recommended
Butt WeldGood
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedExcellent
Forgeability Rating65
Machinability Rating20
Common Fabrication Processes
  • Blanking
  • Coining
  • Coppersmithing
  • Drawing
  • Etching
  • Forming and Bending
  • Heading and Upsetting
  • Hot Forging and Pressing
  • Piercing and Punching
  • Roll Threading and Knurling
  • Shearing
  • Spinning
  • Squeezing and Swaging
  • Stamping
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing7001200
Hot Treatment14001600
Typical uses
Product Category Product Reason Category Reason
ElectricalBus ConductorsConductivity (Electrical)Electrical Conductivity
Bus ConductorsConductivity (Thermal)Thermal Conductivity
BusbarsBrazing CharacteristicsWill not Hydrogen Embrittle during Brazing
BusbarsConductivity (Electrical)Electrical Conductivity
BusbarsConductivity (Thermal)Thermal Conductivity
BusbarsWelding CharacteristicsWill not Hydrogen Embrittle during Welding
Coaxial CablesBrazing CharacteristicsWill not Hydrogen Embrittle during Brazing
Coaxial CablesConductivity (Electrical)Electrical Conductivity
Coaxial CablesWelding CharacteristicsWill not Hydrogen Embrittle during Welding
Copper to Glass Seals in Electronic AppliancesConductivity (Electrical)Electrical Conductivity
Copper to Glass Seals in Electronic AppliancesConductivity (Thermal)Thermal Conductivity
Copper to Glass Seals in Electronic AppliancesMechanical PropertiesDuctility
Electrical ConductorsBrazing CharacteristicsWill not Hydrogen Embrittle during Brazing
Electrical ConductorsConductivity (Electrical)Electrical Conductivity
Electrical ConductorsConductivity (Thermal)Thermal Conductivity
Electrical ConductorsCorrosion ResistanceCorrosion Resistance
Electrical ConductorsWelding CharacteristicsWill not Hydrogen Embrittle during Welding
KlystronsConductivity (Electrical)Electrical Conductivity
KlystronsConductivity (Thermal)Thermal Conductivity
Lead In WireConductivity (Electrical)Electrical Conductivity
Lead In WireConductivity (Thermal)Thermal Conductivity
Lead In WireCorrosion ResistanceCorrosion Resistance
Microwave TubesConductivity (Electrical)Electrical Conductivity
Microwave TubesConductivity (Thermal)Thermal Conductivity
Transistor ComponentsConductivity (Electrical)Electrical Conductivity
Transistor ComponentsConductivity (Thermal)Thermal Conductivity
Wave GuidesConductivity (Electrical)Electrical Conductivity
Wave GuidesConductivity (Thermal)Thermal Conductivity
IndustrialBillet Mold TubeCompositionLow Oxygen Content
Billet Mold TubeConductivity (Electrical)Electrical Conductivity
Billet Mold TubeConductivity (Thermal)Thermal Conductivity
Billet Mold TubeCorrosion ResistanceCorrosion Resistance
Coaxial TubeBrazing CharacteristicsWill not Hydrogen Embrittle during Brazing
Coaxial TubeConductivity (Electrical)Electrical Conductivity
Coaxial TubeWelding CharacteristicsWill not Hydrogen Embrittle during Welding
Extrusion Cans for Powder MetallurgyCompositionLow Oxygen Content
Extrusion Cans for Powder MetallurgyConductivity (Thermal)Thermal Conductivity
Extrusion Cans for Powder MetallurgyForming CharacteristicsLubricity on Dies
Extrusion Cans for Powder MetallurgyWelding CharacteristicsWeldability
Tubing, LP Gas Service
Tubing, Medical Gas- Oxygen
Vacuum SealsForming CharacteristicsFormability
Vacuum SealsPressure TightPressure Tight
OtherTubularCompositionLow Oxygen Content
TubularConductivity (Electrical)Electrical Conductivity
TubularConductivity (Thermal)Thermal Conductivity
TubularCorrosion ResistanceCorrosion Resistance
Applicable Specifications
Form Sub-Form Specific Sub-Form Temper Application System Standard Description
ASTMB224Standard Classification of Coppers
ASTMB577Detection of Cuperous Oxide (Hydrogen Embrittlement Susceptibility) in Copper
BandsProjectile RotatingMILITARYMIL-B-18907BANDS, PROJECTILE ROTATING
Projectile RotatingMILITARYMIL-B-20292BLANKS, ROTATING BAND, FOR PROJECTILES
BarAMS4602COPPER BARS, RODS, AND SHAPES, HARD TEMPER
ASTMB152/B152MCOPPER SHEET, STRIP, PLATE AND ROLLED BAR
Bus BarASTMB187/B187MCOPPER BUS BAR, ROD AND SHAPES AND GENERAL PURPOSE ROD, BAR AND SHAPES
SAEJ461WROUGHT AND CAST COPPER ALLOYS
Bus BarSAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
Bus BarSAEJ463WROUGHT COPPER AND COPPER ALLOYS
Brazing Filler MetalFEDERALQQ-B-650BRAZING ALLOY, COPPER, COPPER-ZINC, AND COPPER-PHOSPHORUS
Bus Bar, Rod and Shapes, General Purpose, same ASMESB187COPPER BUS BAR, ROD AND SHAPES AND GENERAL PURPOSE ROD, BAR AND SHAPES
FittingASMEB16.22WROUGHT COPPER AND COPPER ALLOY SOLDER-JOINT PRESSURE FITTINGS
FoilPrinted CircuitsASTMB451COPPER FOIL, STRIP AND SHEET FOR PRINTED CIRCUITS AND CARRIER TAPES
NipplesASTMB687BRASS, COPPER AND CHROMIUM PLATED PIPE NIPPLES
PipeSeamlessASMESB42SEAMLESS COPPER PIPE, STANDARD SIZES
Bus BarASTMB188SEAMLESS COPPER BUS PIPE AND TUBE
ASTMB42SEAMLESS COPPER PIPE, STANDARD SIZES
ASTMB698COPPER, COPPER ALLOY PLUMBING PIPE AND TUBE
PlateLight Drawn, Light Cold RolledAMS4501COPPER SHEET, STRIP AND PLATE, LIGHT COLD ROLLED
ASTMB152/B152MCOPPER SHEET, STRIP, PLATE AND ROLLED BAR
CladASTMB432COPPER AND COPPER ALLOY CLAD STEEL PLATE
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
Refinery ShapesASTMB170OXYGEN-FREE ELECTROLYTIC COPPER-REFINERY SHAPES
RodAMS4602COPPER BARS, RODS, AND SHAPES, HARD TEMPER
Bus BarASTMB187/B187MCOPPER BUS BAR, ROD AND SHAPES AND GENERAL PURPOSE ROD, BAR AND SHAPES
ASTMB49HOT-ROLLED COPPER ROD REDRAW FOR ELECTRICAL PURPOSES
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
Seamless Condenser Tube & Ferrule StockCondenser TubeASMESB111COPPER AND COPPER ALLOY SEAMLESS CONDENSER TUBES & FERRULE STOCK
ShapesAMS4602COPPER BARS, RODS, AND SHAPES, HARD TEMPER
Bus BarASTMB187/B187MCOPPER BUS BAR, ROD AND SHAPES AND GENERAL PURPOSE ROD, BAR AND SHAPES
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
SheetLight Drawn, Light Cold RolledAMS4501COPPER SHEET, STRIP AND PLATE, LIGHT COLD ROLLED
ASTMB152/B152MCOPPER SHEET, STRIP, PLATE AND ROLLED BAR
Printed CircuitsASTMB451COPPER FOIL, STRIP AND SHEET FOR PRINTED CIRCUITS AND CARRIER TAPES
CladASTMB506COPPER CLAD STAINLESS STEEL SHEET AND STRIP FOR BUILDING CONSTRUCTION
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
Sheet, Strip, Roller Bar & PlateASMESB152COPPER SHEET, STRIP, PLATE, AND ROLLED BAR
StripLight Drawn, Light Cold RolledAMS4501COPPER SHEET, STRIP AND PLATE, LIGHT COLD ROLLED
ASTMB152/B152MCOPPER SHEET, STRIP, PLATE AND ROLLED BAR
Printed CircuitsASTMB451COPPER FOIL, STRIP AND SHEET FOR PRINTED CIRCUITS AND CARRIER TAPES
CladASTMB506COPPER CLAD STAINLESS STEEL SHEET AND STRIP FOR BUILDING CONSTRUCTION
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
TubeFinnedASMESB359COPPER & COPPER ALLOY SEAMLESS CONDENSER & HEAT EXCHANGER TUBES WITH INTEGRAL FINS
U-BendASMESB395U-BEND SEAMLESS COPPER & COPPER ALLOY HEAT EXCHANGER & CONDENSER TUBE
SeamlessASMESB75SEAMLESS COPPER TUBE
Condenser TubeASTMB111/B111MCOPPER AND COPPER ALLOY SEAMLESS CONDENSER TUBES AND FERRULE STOCK
Bus BarASTMB188SEAMLESS COPPER BUS PIPE AND TUBE
ASTMB280SEAMLESS COPPER TUBE FOR AIR CONDITIONING AND REFRIGERATION FIELD SERVICE
FinnedASTMB359/B359MCOPPER AND COPPER-ALLOY SEAMLESS CONDENSER AND HEAT EXCHANGER TUBES WITH INTEGRAL FINS
Rectangular WaveguideASTMB372SEAMLESS COPPER AND COPPER-ALLOY RECTANGULAR WAVEGUIDE TUBE
U-BendASTMB395/B395MU-BEND SEAMLESS COPPER AND COPPER ALLOY HEAT EXCHANGER AND CONDENSER TUBES
WeldedASTMB447WELDED COPPER TUBE
WeldedASTMB640WELDED COPPER AND COPPER ALLOY TUBE FOR AIR CONDITIONING AND REFRIGERATION SERVICE
WeldedASTMB641SEAMLESS AND WELDED COPPER DISTRIBUTION TUBE (TYPE D)
SeamlessASTMB641SEAMLESS AND WELDED COPPER DISTRIBUTION TUBE (TYPE D)
SeamlessAnnealed Tempers, OBright AnnealedASTMB68/B68MSEAMLESS COPPER TUBE, BRIGHT ANNEALED
ASTMB698COPPER, COPPER ALLOY PLUMBING PIPE AND TUBE
WeldedASTMB716WELDED COPPER WATER TUBE
ASTMB743SEAMLESS COPPER TUBE IN COILS
SeamlessASTMB75/B75MSEAMLESS COPPER TUBE
WeldedMILITARYMIL-T-24107TUBE, COPPER, SEAMLESS
SeamlessMILITARYMIL-T-24107TUBE, COPPER, SEAMLESS
SeamlessMILITARYMIL-T-3235TUBE, COPPER, SEAMLESS (FOR TORPEDO USE)
Rectangular WaveguideMILITARYMIL-W-85WAVEGUIDES, RIGID, RECTANGULAR
For Air Conditioning And Refrigeration Field ServiSAEJ461WROUGHT AND CAST COPPER ALLOYS
SeamlessSAEJ461WROUGHT AND CAST COPPER ALLOYS
WeldedSAEJ461WROUGHT AND CAST COPPER ALLOYS
For Air Conditioning And Refrigeration Field ServiSAEJ463WROUGHT COPPER AND COPPER ALLOYS
WeldedSAEJ463WROUGHT COPPER AND COPPER ALLOYS
SeamlessSAEJ463WROUGHT COPPER AND COPPER ALLOYS
Tube, waterASTMB88SEAMLESS COPPER WATER TUBE
ASTMB88MSEAMLESS COPPER WATER TUBE (METRIC)
WireSoftSoft AnnealAMS4701COPPER WIRE, ANNEALED
Hard DrawnHard DrawnASTMB1HARD-DRAWN COPPER WIRE
StrandedASTMB172ROPE-LAY-STANDARD CONDUCTORS WITH BUNCH STRANDED MEMBERS
StrandedASTMB173ROPE-LAY-STRANDED CONDUCTORS WITH CONCENTRIC STRANDED MEMBERS
StrandedASTMB174BUNCH-STRANDED CONDUCTORS
Coated With Lead AlloyASTMB189LEAD-COATED AND LEAD ALLOY COATED SOFT COPPER WIRE FOR ELECTRICAL PURPOSES
Hard DrawnMedium Hard-drawn Electrical WireASTMB2MEDIUM-HARD DRAWN COPPER WIRE
StrandedASTMB226CORED, ANNULAR, CONCENTRIC-LAY-STRANDED COPPER CONDUCTORS
Coated With TinASTMB246TINNED HARD-DRAWN AND MEDIUM HARD-DRAWN COPPER WIRE FOR ELECTRICAL PURPOSES
FlatASTMB272COPPER FLAT PRODUCTS WITH FINISHED (ROLLED OR DRAWN) EDGES (FLAT WIRE AND STRIP)
StrandedASTMB286COPPER CONDUCTORS FOR HOOKUP WIRE IN ELECTRONIC EQUIPMENT
Coated With SilverASTMB298SILVER-COATED SOFT OR ANNEALED COPPER WIRE
SoftSoft AnnealASTMB3SOFT OR ANNEALED COPPER WIRE
Coated With TinASTMB33TINNED SOFT OR ANNEALED COPPER WIRE FOR ELECTRICAL PURPOSES
Coated With NickelASTMB355NICKEL-COATED SOFT OR ANNEALED COPPER WIRE
StrandedASTMB470BONDED COPPER CONDUCTORS FOR USE IN HOOKUP WIRE FOR ELECTRONIC EQUIPMENT
SoftSoft AnnealASTMB48SOFT RECTANGULAR AND SQUARE BARE COPPER WIRE FOR ELECTRICAL CONDUCTORS
StrandedASTMB496COMPACT ROUND CONCENTRIC-LAY-STRANDED COPPER CONDUCTORS
SoftSoft AnnealASTMB738FINE-WIRE BUNCH-STRANDED AND ROPE-LAY BUNCH STRANDED COPPER CONDUCTORS FOR USE AS ELECTRICAL CONDUCT
StrandedASTMB8CONCENTRIC-LAY-STRANDED COPPER CONDUCTORS, HARD, MEDIUM-HARD OR SOFT
SoftSoft AnnealASTMF9ROUND WIRE FOR USE AS GRID SIDE RODS IN ELECTRON TUBES
StrandedFEDERALQQ-B-575BRAID, WIRE (COPPER, TIN-COATED OR SILVER-COATED, TUBULAR OR FLAT)
Hard DrawnHard DrawnFEDERALQQ-W-343WIRE, ELECTRICAL (UNINSULATED)
Hard DrawnMedium Hard-drawn Electrical WireFEDERALQQ-W-343WIRE, ELECTRICAL (UNINSULATED)
SoftSoft AnnealFEDERALQQ-W-343WIRE, ELECTRICAL (UNINSULATED)
MetallizingMILITARYMIL-W-6712WIRE, METALLIZING
Corrosion Properties

No information available.