Find suppliers for this alloy
C10300
| Elements | ||
|---|---|---|
| Cu(1,2) | P | |
|
(1) Cu value includes Ag. (2) Includes P. |
||
| Min (%) | 99.95 | 0.001 |
| Max (%) | 0.005 | |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Rockwell F scale | Rockwell 30T scale | Shear Strength (ksi) |
Torsion Modulus (ksi) |
Fatigue Strength** (ksi) |
Ultimate Tensile Strength in Shear (ksi) |
Section Size (in) |
Cold Work (%) |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | ||||||||||||||
| Flat Products | 1/2 Hard | H02 |
42 Typ |
36 Typ |
14 Typ |
40 Typ |
84 Typ |
50 Typ |
26 Typ |
13 Typ | 0.04 | |||
| 1/4 Hard | H01 |
38 Typ |
30 Typ |
25 Typ |
25 Typ |
70 Typ |
36 Typ |
25 Typ |
0.04 | |||||
| 1/8 Hard | H00 |
36 Typ |
28 Typ |
30 Typ |
10 Typ |
60 Typ |
25 Typ |
25 Typ |
25 Typ |
0.04 | ||||
| 1/8 Hard | H00 |
36 Typ |
28 Typ |
40 Typ |
10 Typ |
60 Typ |
25 Typ |
25 Typ |
0.25 | |||||
| As Hot Rolled | M20 |
32 Typ |
10 Typ |
50 Typ |
40 Typ |
22 Typ |
0.25 | |||||||
| Hard | H04 |
45 Typ |
40 Typ |
20 Typ |
45 Typ |
85 Typ |
26 Typ |
1 | ||||||
| Hard | H04 |
50 Typ |
45 Typ |
12 Typ |
50 Typ |
90 Typ |
28 Typ |
0.25 | ||||||
| Hard | H04 |
50 Typ |
45 Typ |
6 Typ |
50 Typ |
90 Typ |
57 Typ |
28 Typ |
13 Typ | 28 Typ |
0.04 | |||
| Hard | H04 |
45 Typ |
40 Typ |
20 Typ |
1 | |||||||||
| Nominal Grain Size 0.025 mm | OS025 |
34 Typ |
11 Typ |
45 Typ |
45 Typ |
23 Typ |
11 Typ | 0.04 | ||||||
| Nominal Grain Size 0.050 mm | OS050 |
32 Typ |
10 Typ |
50 Typ |
40 Typ |
22 Typ |
0.25 | |||||||
| Nominal Grain Size 0.050 mm | OS050 |
32 Typ |
10 Typ |
45 Typ |
40 Typ |
22 Typ |
0.04 | |||||||
| Pipe | Hard | H04 |
50 Typ |
45 Typ |
10 Typ |
50 Typ |
90 Typ |
28 Typ |
30 | |||||
| Rod | Hard | H04 |
48 Typ |
44 Typ |
16 Typ |
47 Typ |
87 Typ |
27 Typ |
0.25 | 35 | ||||
| Hard | H04 |
55 Typ |
50 Typ |
20 Typ |
60 Typ |
94 Typ |
6.4 Typ | 29 Typ |
0.25 | 40 | ||||
| Hard | H04 |
45 Typ |
40 Typ |
20 Typ |
45 Typ |
85 Typ |
26 Typ |
0.25 | 16 | |||||
| Shapes | Hard | H04 |
40 Typ |
32 Typ |
30 Typ |
35 Typ |
26 Typ |
0.5 | 15 | |||||
| Nominal Grain Size 0.050 mm | OS050 |
32 Typ |
10 Typ |
50 Typ |
40 Typ |
22 Typ |
0.5 | |||||||
| Tube | Hard Drawn | H80 |
55 Typ |
50 Typ |
8 Typ |
60 Typ |
95 Typ |
63 Typ |
29 Typ |
29 Typ |
0.065 | 40 | ||
| Hard Drawn | H80 |
55 Typ |
50 Typ |
20 Typ |
29 Typ |
0.20 | 40 | |||||||
| Light Drawn, Light Cold Rolled | H55 |
40 Typ |
32 Typ |
25 Typ |
35 Typ |
77 Typ |
45 Typ |
26 Typ |
0.065 | 15 | ||||
| Nominal Grain Size 0.025 mm | OS025 |
34 Typ |
11 Typ |
45 Typ |
45 Typ |
23 Typ |
0.065 | |||||||
| Nominal Grain Size 0.050 mm | OS050 |
32 Typ |
10 Typ |
45 Typ |
40 Typ |
22 Typ |
22 Typ |
0.065 | ||||||
| Melting Point - Liquidus°F | 1981 |
|---|---|
| Melting Point - Solidus°F | 1981 |
| Densitylb/cu in. at 68°F | 0.323 |
| Specific Gravity | 8.94 |
| Electrical Conductivity% IACS at 68°F | 99 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 223 |
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 9.4 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 9.6 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.8 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.092 |
| Modulus of Elasticity in Tensionksi | 17000 |
| Modulus of Rigidityksi | 6400 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Fair |
| Gas Shielded Arc Welding | Excellent |
| Coated Metal Arc Welding | Not Recommended |
| Spot Weld | Not Recommended |
| Seam Weld | Not Recommended |
| Butt Weld | Good |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Excellent |
| Forgeability Rating | 65 |
| Machinability Rating | 20 |
Common Fabrication Processes
- Blanking
- Coining
- Coppersmithing
- Drawing
- Etching
- Forming and Bending
- Heading and Upsetting
- Hot Forging and Pressing
- Piercing and Punching
- Roll Threading and Knurling
- Shearing
- Squeezing and Swaging
- Stamping
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 700 | 1200 | ||
| Hot Working Temperature | 1400 | 1600 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Electrical | Applications Requiring High Conductivity | Conductivity (Electrical) | Electrical Conductivity |
| Applications Requiring High Conductivity | Conductivity (Thermal) | Thermal Conductivity | |
| Busbars | Brazing Characteristics | Brazability | |
| Busbars | Conductivity (Electrical) | Electrical Conductivity | |
| Busbars | Conductivity (Thermal) | Thermal Conductivity | |
| Busbars | Corrosion Resistance | Corrosion Resistance | |
| Busbars | Welding Characteristics | Weldability | |
| Clad Products | Conductivity (Electrical) | Electrical Conductivity | |
| Clad Products | Conductivity (Thermal) | Thermal Conductivity | |
| Clad Products | Corrosion Resistance | Corrosion Resistance | |
| Commutators | Conductivity (Electrical) | Electrical Conductivity | |
| Commutators | Conductivity (Thermal) | Thermal Conductivity | |
| Commutators | Corrosion Resistance | Corrosion Resistance | |
| Electrical Conductors | Brazing Characteristics | Brazability | |
| Electrical Conductors | Conductivity (Electrical) | Electrical Conductivity | |
| Electrical Conductors | Conductivity (Thermal) | Thermal Conductivity | |
| Electrical Conductors | Corrosion Resistance | Corrosion Resistance | |
| Electrical Conductors | Welding Characteristics | Weldability | |
| Terminals | Conductivity (Electrical) | Electrical Conductivity | |
| Terminals | Conductivity (Thermal) | Thermal Conductivity | |
| Terminals | Corrosion Resistance | Corrosion Resistance | |
| Thermostatic Control Tubing | Conductivity (Electrical) | Electrical Conductivity | |
| Thermostatic Control Tubing | Conductivity (Thermal) | Thermal Conductivity | |
| Thermostatic Control Tubing | Corrosion Resistance | Corrosion Resistance | |
| Tubular Bus | Conductivity (Electrical) | Electrical Conductivity | |
| Tubular Bus | Conductivity (Thermal) | Thermal Conductivity | |
| Tubular Bus | Corrosion Resistance | Corrosion Resistance | |
| Tubular Bus | Solderability | Solderability | |
| Wave Guide Tubing | Conductivity (Electrical) | Electrical Conductivity | |
| Wave Guide Tubing | Conductivity (Thermal) | Thermal Conductivity | |
| Industrial | Applications Requiring Good Brazing | Brazing Characteristics | Brazability |
| Applications Requiring Good Brazing | Conductivity (Electrical) | Electrical Conductivity | |
| Applications Requiring Good Brazing | Conductivity (Thermal) | Thermal Conductivity | |
| Applications Requiring Good Weldability | Conductivity (Electrical) | Electrical Conductivity | |
| Applications Requiring Good Weldability | Conductivity (Thermal) | Thermal Conductivity | |
| Applications Requiring Good Weldability | Welding Characteristics | Weldability | |
| Billet Mold Tube | Composition | Low Oxygen Content | |
| Billet Mold Tube | Conductivity (Thermal) | Thermal Conductivity | |
| Billet Mold Tube | Corrosion Resistance | Corrosion Resistance | |
| Extrusion Cans for Powder Metallurgy | Composition | Low Oxygen Content | |
| Extrusion Cans for Powder Metallurgy | Conductivity (Thermal) | Thermal Conductivity | |
| Extrusion Cans for Powder Metallurgy | Forming Characteristics | Lubricity on Dies | |
| Extrusion Cans for Powder Metallurgy | Welding Characteristics | Weldability | |
| Pressure Vessels | Brazing Characteristics | Brazability | |
| Pressure Vessels | Corrosion Resistance | Corrosion Resistance | |
| Pressure Vessels | Forming Characteristics | Formability | |
| Pressure Vessels | Solderability | Solderability | |
| Pressure Vessels | Welding Characteristics | Weldability |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| ASTM | B577 | Detection of Cuperous Oxide (Hydrogen Embrittlement Susceptibility) in Copper | |||
| ASTM | B224 | Standard Classification of Coppers | |||
| Bands | Projectile Rotating | MILITARY | MIL-B-20292 | BLANKS, ROTATING BAND, FOR PROJECTILES | |
| Bar | ASTM | B152/B152M | COPPER SHEET, STRIP, PLATE AND ROLLED BAR | ||
| Bus Bar | ASTM | B187/B187M | COPPER BUS BAR, ROD AND SHAPES AND GENERAL PURPOSE ROD, BAR AND SHAPES | ||
| Brazing Filler Metal | FEDERAL | QQ-B-650 | BRAZING ALLOY, COPPER, COPPER-ZINC, AND COPPER-PHOSPHORUS | ||
| Bus Bar, Rod and Shapes, General Purpose, same | ASME | SB187 | COPPER BUS BAR, ROD AND SHAPES AND GENERAL PURPOSE ROD, BAR AND SHAPES | ||
| Condenser & Heat Exchanger Tube with Integral Fins | ASME | SB359 | COPPER & COPPER ALLOY SEAMLESS CONDENSER & HEAT EXCHANGER TUBES WITH INTEGRAL FINS | ||
| Nipples | ASTM | B687 | BRASS, COPPER AND CHROMIUM PLATED PIPE NIPPLES | ||
| Pipe | ASTM | B698 | COPPER, COPPER ALLOY PLUMBING PIPE AND TUBE | ||
| ASTM | B302 | THREADLESS COPPER PIPE | |||
| ASTM | B42 | SEAMLESS COPPER PIPE, STANDARD SIZES | |||
| Bus Bar | ASTM | B188 | SEAMLESS COPPER BUS PIPE AND TUBE | ||
| Pipe, Seamless. Standard Sizes | ASME | SB42 | SEAMLESS COPPER PIPE, STANDARD SIZES | ||
| Plate | ASTM | B432 | COPPER AND COPPER ALLOY CLAD STEEL PLATE | ||
| ASTM | B152/B152M | COPPER SHEET, STRIP, PLATE AND ROLLED BAR | |||
| Refinery Shapes | ASTM | B379 | PHOSPHORIZED COPPERS-REFINERY SHAPES | ||
| Rod | Bus Bar | ASTM | B187/B187M | COPPER BUS BAR, ROD AND SHAPES AND GENERAL PURPOSE ROD, BAR AND SHAPES | |
| Seamless Condenser Tube & Ferrule Stock | ASME | SB111 | COPPER AND COPPER ALLOY SEAMLESS CONDENSER TUBES & FERRULE STOCK | ||
| Seamless Tube | ASME | SB75 | SEAMLESS COPPER TUBE | ||
| Shapes | Bus Bar | ASTM | B187/B187M | COPPER BUS BAR, ROD AND SHAPES AND GENERAL PURPOSE ROD, BAR AND SHAPES | |
| Sheet | ASTM | B152/B152M | COPPER SHEET, STRIP, PLATE AND ROLLED BAR | ||
| Sheet, Strip, Roller Bar & Plate | ASME | SB152 | COPPER SHEET, STRIP, PLATE, AND ROLLED BAR | ||
| Strip | ASTM | B152/B152M | COPPER SHEET, STRIP, PLATE AND ROLLED BAR | ||
| ASTM | B272 | COPPER FLAT PRODUCTS WITH FINISHED (ROLLED OR DRAWN) EDGES (FLAT WIRE AND STRIP) | |||
| Tube | ASTM | B359/B359M | COPPER AND COPPER-ALLOY SEAMLESS CONDENSER AND HEAT EXCHANGER TUBES WITH INTEGRAL FINS | ||
| ASTM | B395/B395M | U-BEND SEAMLESS COPPER AND COPPER ALLOY HEAT EXCHANGER AND CONDENSER TUBES | |||
| Bright Annealed | ASTM | B68/B68M | SEAMLESS COPPER TUBE, BRIGHT ANNEALED | ||
| ASTM | B698 | COPPER, COPPER ALLOY PLUMBING PIPE AND TUBE | |||
| ASTM | B641 | SEAMLESS AND WELDED COPPER DISTRIBUTION TUBE (TYPE D) | |||
| ASTM | B641 | SEAMLESS AND WELDED COPPER DISTRIBUTION TUBE (TYPE D) | |||
| ASTM | B743 | SEAMLESS COPPER TUBE IN COILS | |||
| ASTM | B447 | WELDED COPPER TUBE | |||
| ASTM | B716 | WELDED COPPER WATER TUBE | |||
| Rectangular Waveguide | ASTM | B372 | SEAMLESS COPPER AND COPPER-ALLOY RECTANGULAR WAVEGUIDE TUBE | ||
| Condenser Tube | ASTM | B111/B111M | COPPER AND COPPER ALLOY SEAMLESS CONDENSER TUBES AND FERRULE STOCK | ||
| ASTM | B75/B75M | SEAMLESS COPPER TUBE | |||
| MILITARY | MIL-T-3235 | TUBE, COPPER, SEAMLESS (FOR TORPEDO USE) | |||
| Bus Bar | ASTM | B188 | SEAMLESS COPPER BUS PIPE AND TUBE | ||
| Tubes, Seamless Condenser & Heat Exchanger, U-Bend | ASME | SB395 | U-BEND SEAMLESS COPPER & COPPER ALLOY HEAT EXCHANGER & CONDENSER TUBE | ||
| Wire | ASTM | B272 | COPPER FLAT PRODUCTS WITH FINISHED (ROLLED OR DRAWN) EDGES (FLAT WIRE AND STRIP) |