Find suppliers for this alloyC10300
Chemical Composition
Element
Cu(1,2)P
(1) Cu value includes Ag. (2) Includes P.
Min (%)99.950.001
Max (%)0.005
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell F scale
Rockwell 30T scale
Shear Strength
(ksi)
Torsion Modulus
(ksi)
Fatigue Strength**
(ksi)
Ultimate Tensile Strength in Shear
(ksi)
Section Size
(in)
Cold Work
(%)
Flat Products1/2 HardH0242   Typ
36   Typ
14   Typ
40   Typ
84   Typ
50   Typ
26   Typ
13   Typ
0.04
1/4 HardH0138   Typ
30   Typ
25   Typ
25   Typ
70   Typ
36   Typ
25   Typ
0.04
1/8 HardH0036   Typ
28   Typ
30   Typ
10   Typ
60   Typ
25   Typ
25   Typ
25   Typ
0.04
H0036   Typ
28   Typ
40   Typ
10   Typ
60   Typ
25   Typ
25   Typ
0.25
As Hot RolledM2032   Typ
10   Typ
50   Typ
40   Typ
22   Typ
0.25
HardH0445   Typ
40   Typ
20   Typ
45   Typ
85   Typ
26   Typ
1
H0450   Typ
45   Typ
12   Typ
50   Typ
90   Typ
28   Typ
0.25
H0450   Typ
45   Typ
6   Typ
50   Typ
90   Typ
57   Typ
28   Typ
13   Typ
28   Typ
0.04
H0445   Typ
40   Typ
20   Typ
1
Nominal Grain Size 0.025 mmOS02534   Typ
11   Typ
45   Typ
45   Typ
23   Typ
11   Typ
0.04
Nominal Grain Size 0.050 mmOS05032   Typ
10   Typ
50   Typ
40   Typ
22   Typ
0.25
OS05032   Typ
10   Typ
45   Typ
40   Typ
22   Typ
0.04
PipeHardH0450   Typ
45   Typ
10   Typ
50   Typ
90   Typ
28   Typ
30
RodHardH0448   Typ
44   Typ
16   Typ
47   Typ
87   Typ
27   Typ
0.2535
H0455   Typ
50   Typ
20   Typ
60   Typ
94   Typ
6.4   Typ
29   Typ
0.2540
H0445   Typ
40   Typ
20   Typ
45   Typ
85   Typ
26   Typ
0.2516
ShapesHardH0440   Typ
32   Typ
30   Typ
35   Typ
26   Typ
0.515
Nominal Grain Size 0.050 mmOS05032   Typ
10   Typ
50   Typ
40   Typ
22   Typ
0.5
TubeHard DrawnH8055   Typ
50   Typ
8   Typ
60   Typ
95   Typ
63   Typ
29   Typ
29   Typ
0.06540
H8055   Typ
50   Typ
20   Typ
29   Typ
0.2040
Light Drawn, Light Cold RolledH5540   Typ
32   Typ
25   Typ
35   Typ
77   Typ
45   Typ
26   Typ
0.06515
Nominal Grain Size 0.025 mmOS02534   Typ
11   Typ
45   Typ
45   Typ
23   Typ
0.065
Nominal Grain Size 0.050 mmOS05032   Typ
10   Typ
45   Typ
40   Typ
22   Typ
22   Typ
0.065
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
Melting Point - Liquidus°F1981
Melting Point - Solidus°F1981
Densitylb/cu in. at 68°F0.323
Specific Gravity8.94
Electrical Conductivity% IACS at 68°F99
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F223
Coefficient of Thermal Expansion 68-21210⁻⁶ per °F (68 – 212°F)9.4
Coefficient of Thermal Expansion 68-39210⁻⁶ per °F (68 – 392°F)9.6
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)9.8
Specific Heat CapacityBtu/ lb /°F at 68°F0.092
Modulus of Elasticity in Tensionksi17000
Modulus of Rigidityksi6400
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingFair
Gas Shielded Arc WeldingExcellent
Coated Metal Arc WeldingNot Recommended
Spot WeldNot Recommended
Seam WeldNot Recommended
Butt WeldGood
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedExcellent
Forgeability Rating65
Machinability Rating20
Common Fabrication Processes
  • Blanking
  • Coining
  • Coppersmithing
  • Drawing
  • Etching
  • Forming and Bending
  • Heading and Upsetting
  • Hot Forging and Pressing
  • Piercing and Punching
  • Roll Threading and Knurling
  • Shearing
  • Squeezing and Swaging
  • Stamping
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing7001200
Hot Treatment14001600
Typical uses
Product Category Product Reason Category Reason
ElectricalApplications Requiring High ConductivityConductivity (Electrical)Electrical Conductivity
Applications Requiring High ConductivityConductivity (Thermal)Thermal Conductivity
BusbarsBrazing CharacteristicsBrazability
BusbarsConductivity (Electrical)Electrical Conductivity
BusbarsConductivity (Thermal)Thermal Conductivity
BusbarsCorrosion ResistanceCorrosion Resistance
BusbarsWelding CharacteristicsWeldability
Clad ProductsConductivity (Electrical)Electrical Conductivity
Clad ProductsConductivity (Thermal)Thermal Conductivity
Clad ProductsCorrosion ResistanceCorrosion Resistance
CommutatorsConductivity (Electrical)Electrical Conductivity
CommutatorsConductivity (Thermal)Thermal Conductivity
CommutatorsCorrosion ResistanceCorrosion Resistance
Electrical ConductorsBrazing CharacteristicsBrazability
Electrical ConductorsConductivity (Electrical)Electrical Conductivity
Electrical ConductorsConductivity (Thermal)Thermal Conductivity
Electrical ConductorsCorrosion ResistanceCorrosion Resistance
Electrical ConductorsWelding CharacteristicsWeldability
TerminalsConductivity (Electrical)Electrical Conductivity
TerminalsConductivity (Thermal)Thermal Conductivity
TerminalsCorrosion ResistanceCorrosion Resistance
Thermostatic Control TubingConductivity (Electrical)Electrical Conductivity
Thermostatic Control TubingConductivity (Thermal)Thermal Conductivity
Thermostatic Control TubingCorrosion ResistanceCorrosion Resistance
Tubular BusConductivity (Electrical)Electrical Conductivity
Tubular BusConductivity (Thermal)Thermal Conductivity
Tubular BusCorrosion ResistanceCorrosion Resistance
Tubular BusSolderabilitySolderability
Wave Guide TubingConductivity (Electrical)Electrical Conductivity
Wave Guide TubingConductivity (Thermal)Thermal Conductivity
IndustrialApplications Requiring Good BrazingBrazing CharacteristicsBrazability
Applications Requiring Good BrazingConductivity (Electrical)Electrical Conductivity
Applications Requiring Good BrazingConductivity (Thermal)Thermal Conductivity
Applications Requiring Good WeldabilityConductivity (Electrical)Electrical Conductivity
Applications Requiring Good WeldabilityConductivity (Thermal)Thermal Conductivity
Applications Requiring Good WeldabilityWelding CharacteristicsWeldability
Billet Mold TubeCompositionLow Oxygen Content
Billet Mold TubeConductivity (Thermal)Thermal Conductivity
Billet Mold TubeCorrosion ResistanceCorrosion Resistance
Extrusion Cans for Powder MetallurgyCompositionLow Oxygen Content
Extrusion Cans for Powder MetallurgyConductivity (Thermal)Thermal Conductivity
Extrusion Cans for Powder MetallurgyForming CharacteristicsLubricity on Dies
Extrusion Cans for Powder MetallurgyWelding CharacteristicsWeldability
Pressure VesselsBrazing CharacteristicsBrazability
Pressure VesselsCorrosion ResistanceCorrosion Resistance
Pressure VesselsForming CharacteristicsFormability
Pressure VesselsSolderabilitySolderability
Pressure VesselsWelding CharacteristicsWeldability
Applicable Specifications
Form Specific Sub-Form Temper Application System Standard Description
ASTMB224Standard Classification of Coppers
ASTMB577Detection of Cuperous Oxide (Hydrogen Embrittlement Susceptibility) in Copper
BandsProjectile RotatingMILITARYMIL-B-20292BLANKS, ROTATING BAND, FOR PROJECTILES
BarASTMB152/B152MCOPPER SHEET, STRIP, PLATE AND ROLLED BAR
Bus BarASTMB187/B187MCOPPER BUS BAR, ROD AND SHAPES AND GENERAL PURPOSE ROD, BAR AND SHAPES
Brazing Filler MetalFEDERALQQ-B-650BRAZING ALLOY, COPPER, COPPER-ZINC, AND COPPER-PHOSPHORUS
Bus Bar, Rod and Shapes, General Purpose, same ASMESB187COPPER BUS BAR, ROD AND SHAPES AND GENERAL PURPOSE ROD, BAR AND SHAPES
Condenser & Heat Exchanger Tube with Integral FinsASMESB359COPPER & COPPER ALLOY SEAMLESS CONDENSER & HEAT EXCHANGER TUBES WITH INTEGRAL FINS
NipplesASTMB687BRASS, COPPER AND CHROMIUM PLATED PIPE NIPPLES
PipeBus BarASTMB188SEAMLESS COPPER BUS PIPE AND TUBE
Threadless(Seamless)ASTMB302THREADLESS COPPER PIPE
ASTMB42SEAMLESS COPPER PIPE, STANDARD SIZES
ASTMB698COPPER, COPPER ALLOY PLUMBING PIPE AND TUBE
Pipe, Seamless. Standard SizesASMESB42SEAMLESS COPPER PIPE, STANDARD SIZES
PlateASTMB152/B152MCOPPER SHEET, STRIP, PLATE AND ROLLED BAR
CladASTMB432COPPER AND COPPER ALLOY CLAD STEEL PLATE
Refinery ShapesASTMB379PHOSPHORIZED COPPERS-REFINERY SHAPES
RodBus BarASTMB187/B187MCOPPER BUS BAR, ROD AND SHAPES AND GENERAL PURPOSE ROD, BAR AND SHAPES
Seamless Condenser Tube & Ferrule StockASMESB111COPPER AND COPPER ALLOY SEAMLESS CONDENSER TUBES & FERRULE STOCK
Seamless TubeASMESB75SEAMLESS COPPER TUBE
ShapesBus BarASTMB187/B187MCOPPER BUS BAR, ROD AND SHAPES AND GENERAL PURPOSE ROD, BAR AND SHAPES
SheetASTMB152/B152MCOPPER SHEET, STRIP, PLATE AND ROLLED BAR
Sheet, Strip, Roller Bar & PlateASMESB152COPPER SHEET, STRIP, PLATE, AND ROLLED BAR
StripASTMB152/B152MCOPPER SHEET, STRIP, PLATE AND ROLLED BAR
ASTMB272COPPER FLAT PRODUCTS WITH FINISHED (ROLLED OR DRAWN) EDGES (FLAT WIRE AND STRIP)
TubeCondenser TubeASTMB111/B111MCOPPER AND COPPER ALLOY SEAMLESS CONDENSER TUBES AND FERRULE STOCK
Bus BarASTMB188SEAMLESS COPPER BUS PIPE AND TUBE
FinnedASTMB359/B359MCOPPER AND COPPER-ALLOY SEAMLESS CONDENSER AND HEAT EXCHANGER TUBES WITH INTEGRAL FINS
Rectangular WaveguideASTMB372SEAMLESS COPPER AND COPPER-ALLOY RECTANGULAR WAVEGUIDE TUBE
U-BendASTMB395/B395MU-BEND SEAMLESS COPPER AND COPPER ALLOY HEAT EXCHANGER AND CONDENSER TUBES
WeldedASTMB447WELDED COPPER TUBE
WeldedASTMB641SEAMLESS AND WELDED COPPER DISTRIBUTION TUBE (TYPE D)
SeamlessASTMB641SEAMLESS AND WELDED COPPER DISTRIBUTION TUBE (TYPE D)
SeamlessAnnealed Tempers, OBright AnnealedASTMB68/B68MSEAMLESS COPPER TUBE, BRIGHT ANNEALED
ASTMB698COPPER, COPPER ALLOY PLUMBING PIPE AND TUBE
WeldedASTMB716WELDED COPPER WATER TUBE
ASTMB743SEAMLESS COPPER TUBE IN COILS
SeamlessASTMB75/B75MSEAMLESS COPPER TUBE
SeamlessMILITARYMIL-T-3235TUBE, COPPER, SEAMLESS (FOR TORPEDO USE)
Tubes, Seamless Condenser & Heat Exchanger, U-BendASMESB395U-BEND SEAMLESS COPPER & COPPER ALLOY HEAT EXCHANGER & CONDENSER TUBE
WireFlatASTMB272COPPER FLAT PRODUCTS WITH FINISHED (ROLLED OR DRAWN) EDGES (FLAT WIRE AND STRIP)
Corrosion Properties

No information available.