Find suppliers for this alloyC10400
Chemical Composition
Element
Cu(1,2,3)Ag(4)O
(1) This is a high conductivity copper which has, in the annealed condition a minimum conductivity of 100% IACS except for Alloy C10100 which has a minimum conductivity of 101% IACS. (2) Cu value includes Ag. (3) Cu is determined by the difference between the impurity total and 100%. (4) Ag 0.027% min is the equivalent of, Ag 8 Troy Oz min.
Min (%)99.950.027
Max (%)0.0010
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell F scale
Rockwell 30T scale
Shear Strength
(ksi)
Section Size
(in)
Cold Work
(%)
Flat Products1/2 HardH0242   Typ
36   Typ
14   Typ
40   Typ
84   Typ
50   Typ
26   Typ
0.04
1/4 HardH0138   Typ
30   Typ
35   Typ
25   Typ
70   Typ
25   Typ
0.25
H0138   Typ
30   Typ
25   Typ
25   Typ
70   Typ
36   Typ
25   Typ
0.04
1/8 HardH0036   Typ
28   Typ
40   Typ
10   Typ
60   Typ
25   Typ
0.25
H0036   Typ
28   Typ
30   Typ
10   Typ
60   Typ
25   Typ
25   Typ
0.04
As Hot RolledM2034   Typ
10   Typ
45   Typ
45   Typ
23   Typ
0.04
M2032   Typ
10   Typ
50   Typ
40   Typ
22   Typ
0.25
Extra SpringH1057   Typ
53   Typ
4   Typ
62   Typ
95   Typ
64   Typ
29   Typ
0.04
HardH0450   Typ
45   Typ
12   Typ
50   Typ
90   Typ
28   Typ
0.25
H0445   Typ
40   Typ
20   Typ
45   Typ
85   Typ
26   Typ
1
H0450   Typ
45   Typ
6   Typ
50   Typ
90   Typ
57   Typ
28   Typ
0.04
Nominal Grain Size 0.025 mmOS02534   Typ
11   Typ
45   Typ
45   Typ
23   Typ
0.04
Nominal Grain Size 0.050 mmOS05032   Typ
10   Typ
50   Typ
40   Typ
22   Typ
0.25
SpringH0855   Typ
50   Typ
4   Typ
60   Typ
94   Typ
63   Typ
29   Typ
0.04
RodAs Hot RolledM2032   Typ
10   Typ
55   Typ
40   Typ
22   Typ
1
HardH0455   Typ
50   Typ
10   Typ
60   Typ
94   Typ
29   Typ
0.2540
H0448   Typ
44   Typ
16   Typ
47   Typ
87   Typ
27   Typ
135
H0445   Typ
40   Typ
20   Typ
45   Typ
85   Typ
26   Typ
216
Nominal Grain Size 0.050 mmOS05032   Typ
10   Typ
55   Typ
40   Typ
22   Typ
1
ShapesAs Hot ExtrudedM3032   Typ
10   Typ
50   Typ
40   Typ
22   Typ
0.5
As Hot RolledM2032   Typ
10   Typ
50   Typ
40   Typ
22   Typ
0.5
HardH0440   Typ
32   Typ
30   Typ
35   Typ
26   Typ
0.515
Nominal Grain Size 0.050 mmOS05032   Typ
10   Typ
50   Typ
40   Typ
22   Typ
0.5
TubeHard DrawnH8055   Typ
50   Typ
8   Typ
60   Typ
95   Typ
62   Typ
29   Typ
0.06540
Light Drawn, Light Cold RolledH5540   Typ
32   Typ
25   Typ
35   Typ
77   Typ
45   Typ
26   Typ
0.06515
Nominal Grain Size 0.025 mmOS02534   Typ
11   Typ
45   Typ
45   Typ
23   Typ
0.065
Nominal Grain Size 0.050 mmOS05032   Typ
10   Typ
45   Typ
40   Typ
22   Typ
0.065
WireHardH0455   Typ
1.5   Typ
29   Typ
0.08
Nominal Grain Size 0.050 mmOS05035   Typ
35   Typ
24   Typ
0.08
SpringH0866   Typ
1.5   Typ
33   Typ
0.08
* Measured at room temperature, 68°F (20°C).
Physical Properties
(1) Volume and weight basis.
Melting Point - Liquidus°F1981
Melting Point - Solidus°F1981
Densitylb/cu in. at 68°F0.323
Specific Gravity8.94
Electrical Conductivity% IACS at 68°F100(1)
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F224
Coefficient of Thermal Expansion 68-21210⁻⁶ per °F (68 – 212°F)9.4
Coefficient of Thermal Expansion 68-39210⁻⁶ per °F (68 – 392°F)9.6
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)9.8
Modulus of Elasticity in Tensionksi17000
Modulus of Rigidityksi6400
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingFair
Gas Shielded Arc WeldingGood
Coated Metal Arc WeldingNot Recommended
Spot WeldNot Recommended
Seam WeldNot Recommended
Butt WeldGood
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedExcellent
Forgeability Rating65
Machinability Rating20
Common Fabrication Processes
  • Blanking
  • Coining
  • Coppersmithing
  • Drawing
  • Etching
  • Forming and Bending
  • Heading and Upsetting
  • Hot Forging and Pressing
  • Piercing and Punching
  • Roll Threading and Knurling
  • Shearing
  • Spinning
  • Squeezing and Swaging
  • Stamping
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing9001400
Hot Treatment14001600
Typical uses
Product Category Product Reason Category Reason
AutomotiveGasketsConductivity (Thermal)Thermal Conductivity
GasketsForming CharacteristicsFormability
GasketsMechanical PropertiesDuctility
GasketsPressure TightPressure Tight
RadiatorsBrazing CharacteristicsBrazability
RadiatorsConductivity (Thermal)Thermal Conductivity
RadiatorsCorrosion ResistanceCorrosion Resistance
RadiatorsMechanical PropertiesCreep Resistance
RadiatorsSolderabilitySolderability
ElectricalBusbarsConductivity (Electrical)Electrical Conductivity
BusbarsConductivity (Thermal)Thermal Conductivity
BusbarsCorrosion ResistanceCorrosion Resistance
BusbarsSoftening ResistanceResistance to Thermal Softening
BusbarsSolderabilitySolderability
BusbarsWelding CharacteristicsWeldability
Commutator SegmentsConductivity (Electrical)Electrical Conductivity
Commutator SegmentsConductivity (Thermal)Thermal Conductivity
Commutator SegmentsCorrosion ResistanceCorrosion Resistance
Commutator SegmentsSoftening ResistanceResistance to Thermal Softening
Commutator SegmentsSolderabilitySolderability
Commutator SegmentsWelding CharacteristicsWeldability
Conductivity WireConductivity (Electrical)Electrical Conductivity
Conductivity WireConductivity (Thermal)Thermal Conductivity
ContactsConductivity (Electrical)Electrical Conductivity
ContactsConductivity (Thermal)Thermal Conductivity
ContactsCorrosion ResistanceCorrosion Resistance
ContactsSolderabilitySolderability
Printed Circuit FoilConductivity (Electrical)Electrical Conductivity
Printed Circuit FoilConductivity (Thermal)Thermal Conductivity
Printed Circuit FoilCorrosion ResistanceCorrosion Resistance
Printed Circuit FoilForming CharacteristicsFormability
Printed Circuit FoilSolderabilitySolderability
Radio PartsConductivity (Electrical)Electrical Conductivity
Radio PartsConductivity (Thermal)Thermal Conductivity
Radio PartsCorrosion ResistanceCorrosion Resistance
Radio PartsSolderabilitySolderability
SwitchesConductivity (Electrical)Electrical Conductivity
SwitchesConductivity (Thermal)Thermal Conductivity
SwitchesCorrosion ResistanceCorrosion Resistance
SwitchesSolderabilitySolderability
Terminal ConnectorsConductivity (Electrical)Electrical Conductivity
Terminal ConnectorsConductivity (Thermal)Thermal Conductivity
Terminal ConnectorsCorrosion ResistanceCorrosion Resistance
Terminal ConnectorsSoftening ResistanceResistance to Thermal Softening
Terminal ConnectorsSolderabilitySolderability
Terminal ConnectorsWelding CharacteristicsWeldability
WindingsConductivity (Electrical)Electrical Conductivity
WindingsConductivity (Thermal)Thermal Conductivity
WindingsCorrosion ResistanceCorrosion Resistance
WindingsMechanical PropertiesCreep Resistance
WindingsSolderabilitySolderability
IndustrialApplications Requiring Brazing in Hydrogen AtmosphereBrazing CharacteristicsWill not Hydrogen Embrittle during Brazing
Chemical Process EquipmentConductivity (Electrical)Electrical Conductivity
Chemical Process EquipmentConductivity (Thermal)Thermal Conductivity
Chemical Process EquipmentCorrosion ResistanceCorrosion Resistance
Clad MetalsConductivity (Electrical)Electrical Conductivity
Clad MetalsCorrosion ResistanceCorrosion Resistance
Clad MetalsMechanical PropertiesVery High Strength
Heat ExchangersBrazing CharacteristicsBrazability
Heat ExchangersConductivity (Thermal)Thermal Conductivity
Heat ExchangersCorrosion ResistanceCorrosion Resistance
Heat ExchangersSoftening ResistanceResistance to Thermal Softening
Printing RollsCorrosion ResistanceCorrosion Resistance
Printing RollsForming CharacteristicsFormability
Applicable Specifications
Form Sub-Form Specific Sub-Form Temper Application System Standard Description
ASTMB224Standard Classification of Coppers
ASTMB577Detection of Cuperous Oxide (Hydrogen Embrittlement Susceptibility) in Copper
BandsProjectile RotatingMILITARYMIL-B-20292BLANKS, ROTATING BAND, FOR PROJECTILES
Brazing Filler MetalFEDERALQQ-B-650BRAZING ALLOY, COPPER, COPPER-ZINC, AND COPPER-PHOSPHORUS
Bus Bar, Rod and Shapes, General Purpose, same ASMESB187COPPER BUS BAR, ROD AND SHAPES AND GENERAL PURPOSE ROD, BAR AND SHAPES
Bus BarASTMB187/B187MCOPPER BUS BAR, ROD AND SHAPES AND GENERAL PURPOSE ROD, BAR AND SHAPES
PipeBus BarASTMB188SEAMLESS COPPER BUS PIPE AND TUBE
Refinery ShapesASTMB170OXYGEN-FREE ELECTROLYTIC COPPER-REFINERY SHAPES
SheetCladASTMB506COPPER CLAD STAINLESS STEEL SHEET AND STRIP FOR BUILDING CONSTRUCTION
Sheet, Strip, Roller Bar & PlateASMESB152COPPER SHEET, STRIP, PLATE, AND ROLLED BAR
ASTMB152/B152MCOPPER SHEET, STRIP, PLATE AND ROLLED BAR
StripCladASTMB506COPPER CLAD STAINLESS STEEL SHEET AND STRIP FOR BUILDING CONSTRUCTION
TubeBus BarASTMB188SEAMLESS COPPER BUS PIPE AND TUBE
WireHard DrawnHard DrawnASTMB1HARD-DRAWN COPPER WIRE
Coated With Lead AlloyASTMB189LEAD-COATED AND LEAD ALLOY COATED SOFT COPPER WIRE FOR ELECTRICAL PURPOSES
Hard DrawnMedium Hard-drawn Electrical WireASTMB2MEDIUM-HARD DRAWN COPPER WIRE
Coated With TinASTMB246TINNED HARD-DRAWN AND MEDIUM HARD-DRAWN COPPER WIRE FOR ELECTRICAL PURPOSES
Coated With SilverASTMB298SILVER-COATED SOFT OR ANNEALED COPPER WIRE
SoftSoft AnnealASTMB3SOFT OR ANNEALED COPPER WIRE
Coated With NickelASTMB355NICKEL-COATED SOFT OR ANNEALED COPPER WIRE
Hard DrawnMedium Hard-drawn Electrical WireFEDERALQQ-W-343WIRE, ELECTRICAL (UNINSULATED)
SoftSoft AnnealFEDERALQQ-W-343WIRE, ELECTRICAL (UNINSULATED)
Hard DrawnHard DrawnFEDERALQQ-W-343WIRE, ELECTRICAL (UNINSULATED)
Corrosion Properties

No information available.