Find suppliers for this alloyC10800
Chemical Composition
Element
Cu(1,2)P
(1) Includes P. (2) Cu value includes Ag.
Min (%)99.950.005
Max (%)0.012
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell F scale
Rockwell 30T scale
Shear Strength
(ksi)
Torsion Modulus
(ksi)
Fatigue Strength**
(ksi)
Ultimate Tensile Strength in Shear
(ksi)
Section Size
(in)
Cold Work
(%)
Flat Products1/2 HardH0242   Typ
36   Typ
14   Typ
40   Typ
84   Typ
50   Typ
26   Typ
13   Typ
0.04
1/4 HardH0138   Typ
30   Typ
25   Typ
25   Typ
70   Typ
36   Typ
25   Typ
0.04
1/8 HardH0036   Typ
28   Typ
40   Typ
10   Typ
60   Typ
25   Typ
25   Typ
0.25
H0036   Typ
28   Typ
30   Typ
10   Typ
60   Typ
25   Typ
25   Typ
25   Typ
0.04
As Hot RolledM2032   Typ
10   Typ
50   Typ
40   Typ
22   Typ
0.25
HardH0445   Typ
40   Typ
20   Typ
45   Typ
85   Typ
26   Typ
1
H0450   Typ
45   Typ
6   Typ
12   Typ
50   Typ
90   Typ
28   Typ
28   Typ
0.25
H0450   Typ
45   Typ
6   Typ
50   Typ
90   Typ
57   Typ
28   Typ
13   Typ
0.04
Nominal Grain Size 0.025 mmOS02534   Typ
11   Typ
45   Typ
45   Typ
23   Typ
11   Typ
0.04
Nominal Grain Size 0.050 mmOS05032   Typ
10   Typ
50   Typ
40   Typ
22   Typ
0.25
SpringH0855   Typ
50   Typ
4   Typ
60   Typ
94   Typ
63   Typ
29   Typ
14   Typ
0.04
PipeHardH0450   Typ
45   Typ
10   Typ
50   Typ
90   Typ
18   Typ
30
RodHardH0448   Typ
44   Typ
16   Typ
47   Typ
87   Typ
27   Typ
17   Typ
135
H0445   Typ
40   Typ
20   Typ
45   Typ
85   Typ
6.4   Typ
26   Typ
216
H0455   Typ
50   Typ
20   Typ
60   Typ
94   Typ
29   Typ
0.2540
TubeDrawn General PurposeH5836   Min for Standard
30   Min for Standard
30   Min for Standard
Hard DrawnH8055   Typ
50   Typ
8   Typ
60   Typ
95   Typ
63   Typ
29   Typ
0.06540
H8055   Typ
50   Typ
8   Typ
29   Typ
40
Light Drawn, Light Cold RolledH5540   Typ
32   Typ
25   Typ
35   Typ
77   Typ
45   Typ
26   Typ
0.06515
Nominal Grain Size 0.025 mmOS02534   Typ
11   Typ
45   Typ
45   Typ
23   Typ
0.065
Nominal Grain Size 0.050 mmOS05032   Typ
10   Typ
45   Typ
40   Typ
22   Typ
0.065
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
Melting Point - Liquidus°F1981
Melting Point - Solidus°F1981
Densitylb/cu in. at 68°F0.323
Specific Gravity8.94
Electrical Conductivity% IACS at 68°F92
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F202
Coefficient of Thermal Expansion 68-21210⁻⁶ per °F (68 – 212°F)9.4
Coefficient of Thermal Expansion 68-39210⁻⁶ per °F (68 – 392°F)9.6
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)9.8
Specific Heat CapacityBtu/ lb /°F at 68°F0.092
Modulus of Elasticity in Tensionksi17000
Modulus of Rigidityksi6400
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingGood
Gas Shielded Arc WeldingExcellent
Coated Metal Arc WeldingNot Recommended
Spot WeldNot Recommended
Seam WeldNot Recommended
Butt WeldGood
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedExcellent
Forgeability Rating65
Machinability Rating20
Common Fabrication Processes
  • Blanking
  • Coining
  • Coppersmithing
  • Drawing
  • Etching
  • Forming and Bending
  • Heading and Upsetting
  • Hot Forging and Pressing
  • Piercing and Punching
  • Roll Threading and Knurling
  • Shearing
  • Spinning
  • Squeezing and Swaging
  • Stamping
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing7001200
Hot Treatment14001600
Typical uses
Product Category Product Reason Category Reason
AutomotiveAir LinesBrazing CharacteristicsBrazability
Air LinesConductivity (Thermal)Thermal Conductivity
Air LinesCorrosion ResistanceCorrosion Resistance
Air LinesForming CharacteristicsFormability
Air LinesPressure TightPressure Tight
Air LinesSolderabilitySolderability
Gasoline LinesCorrosion ResistanceCorrosion Resistance
Gasoline LinesForming CharacteristicsFormability
Gasoline LinesPressure TightPressure Tight
Gasoline LinesSolderabilitySolderability
Hydraulic LinesCorrosion ResistanceCorrosion Resistance
Hydraulic LinesForming CharacteristicsFormability
Hydraulic LinesPressure TightPressure Tight
Hydraulic LinesSolderabilitySolderability
Oil CoolersCorrosion ResistanceCorrosion Resistance
Oil CoolersSolderabilitySolderability
Oil LinesCorrosion ResistanceCorrosion Resistance
Oil LinesSolderabilitySolderability
ThermostatsBrazing CharacteristicsBrazability
ThermostatsConductivity (Thermal)Thermal Conductivity
ThermostatsCorrosion ResistanceCorrosion Resistance
ThermostatsForming CharacteristicsFormability
BuildingGas Lines and UnitsConductivity (Thermal)Thermal Conductivity
Gas Lines and UnitsCorrosion ResistanceCorrosion Resistance
Gas Lines and UnitsForming CharacteristicsFormability
Gas Lines and UnitsPressure TightPressure Tight
Gas Lines and UnitsSolderabilitySolderability
Heater LinesConductivity (Thermal)Thermal Conductivity
Heater LinesCorrosion ResistanceCorrosion Resistance
Heater LinesForming CharacteristicsFormability
Heater LinesPressure TightPressure Tight
Heater LinesSolderabilitySolderability
Heater UnitsConductivity (Thermal)Thermal Conductivity
Heater UnitsCorrosion ResistanceCorrosion Resistance
Heater UnitsForming CharacteristicsFormability
Heater UnitsPressure TightPressure Tight
Heater UnitsSolderabilitySolderability
Oil Burner TubesCorrosion ResistanceCorrosion Resistance
Oil Burner TubesSolderabilitySolderability
Plumbing PipeBrazing CharacteristicsBrazability
Plumbing PipeCorrosion ResistanceCorrosion Resistance
Plumbing PipeForming CharacteristicsFormability
Plumbing PipeSolderabilitySolderability
Plumbing TubeBrazing CharacteristicsBrazability
Plumbing TubeCorrosion ResistanceCorrosion Resistance
Plumbing TubeForming CharacteristicsFormability
Plumbing TubeSolderabilitySolderability
ConsumerAir ConditionersBrazing CharacteristicsBrazability
Air ConditionersConductivity (Thermal)Thermal Conductivity
Air ConditionersCorrosion ResistanceCorrosion Resistance
Air ConditionersForming CharacteristicsFormability
Air ConditionersPressure TightPressure Tight
RefrigeratorsConductivity (Thermal)Thermal Conductivity
RefrigeratorsCorrosion ResistanceCorrosion Resistance
RefrigeratorsForming CharacteristicsFormability
RefrigeratorsPressure TightPressure Tight
RefrigeratorsSolderabilitySolderability
ElectricalClad ProductsConductivity (Electrical)Electrical Conductivity
Clad ProductsConductivity (Thermal)Thermal Conductivity
Clad ProductsCorrosion ResistanceCorrosion Resistance
CommutatorsConductivity (Electrical)Electrical Conductivity
CommutatorsConductivity (Thermal)Thermal Conductivity
CommutatorsCorrosion ResistanceCorrosion Resistance
Thermostatic Control TubingConductivity (Electrical)Electrical Conductivity
Thermostatic Control TubingConductivity (Thermal)Thermal Conductivity
IndustrialAir Conditioning TubingBrazing CharacteristicsBrazability
Air Conditioning TubingConductivity (Thermal)Thermal Conductivity
Air Conditioning TubingCorrosion ResistanceCorrosion Resistance
Air Conditioning TubingForming CharacteristicsFormability
Air Conditioning TubingPressure TightPressure Tight
Brewery TubesBrazing CharacteristicsBrazability
Brewery TubesConductivity (Thermal)Thermal Conductivity
Brewery TubesCorrosion ResistanceCorrosion Resistance
Brewery TubesForming CharacteristicsFormability
Brewery TubesPressure TightPressure Tight
Brewery TubesSolderabilitySolderability
Condenser TubesBrazing CharacteristicsBrazability
Condenser TubesConductivity (Thermal)Thermal Conductivity
Condenser TubesCorrosion ResistanceCorrosion Resistance
Condenser TubesForming CharacteristicsFormability
Condenser TubesPressure TightPressure Tight
Condenser TubesSolderabilitySolderability
Dairy TubesBrazing CharacteristicsBrazability
Dairy TubesConductivity (Thermal)Thermal Conductivity
Dairy TubesCorrosion ResistanceCorrosion Resistance
Dairy TubesForming CharacteristicsFormability
Dairy TubesPressure TightPressure Tight
Dairy TubesSolderabilitySolderability
Distiller TubesBrazing CharacteristicsBrazability
Distiller TubesConductivity (Thermal)Thermal Conductivity
Distiller TubesCorrosion ResistanceCorrosion Resistance
Distiller TubesForming CharacteristicsFormability
Distiller TubesPressure TightPressure Tight
Distiller TubesSolderabilitySolderability
Gage LinesBrazing CharacteristicsBrazability
Gage LinesConductivity (Thermal)Thermal Conductivity
Gage LinesCorrosion ResistanceCorrosion Resistance
Gage LinesForming CharacteristicsFormability
Gage LinesPressure TightPressure Tight
Gage LinesSolderabilitySolderability
Heat Exchanger TubesConductivity (Thermal)Thermal Conductivity
Heat Exchanger TubesCorrosion ResistanceCorrosion Resistance
Heat Exchanger TubesForming CharacteristicsFormability
Heat Exchanger TubesPressure TightPressure Tight
Heat Exchanger TubesSolderabilitySolderability
KettlesAppearanceAppearance
KettlesConductivity (Thermal)Thermal Conductivity
KettlesCorrosion ResistanceCorrosion Resistance
Paper LinesConductivity (Thermal)Thermal Conductivity
Paper LinesCorrosion ResistanceCorrosion Resistance
Plate for Welded Continuous Cast MoldsConductivity (Thermal)High Thermal Conductivity
Plate for Welded Continuous Cast MoldsCorrosion ResistanceCorrosion Resistance
Plate for Welded Continuous Cast MoldsWelding CharacteristicsWeldability
Pulp LinesConductivity (Thermal)Thermal Conductivity
Pulp LinesCorrosion ResistanceCorrosion Resistance
RefrigeratorsConductivity (Thermal)Thermal Conductivity
RefrigeratorsCorrosion ResistanceCorrosion Resistance
RefrigeratorsForming CharacteristicsFormability
RefrigeratorsPressure TightPressure Tight
RefrigeratorsSolderabilitySolderability
Rotating BandsConductivity (Thermal)Thermal Conductivity
Rotating BandsCorrosion ResistanceCorrosion Resistance
Steam LinesConductivity (Thermal)Thermal Conductivity
Steam LinesCorrosion ResistanceCorrosion Resistance
Steam LinesMechanical PropertiesCreep Resistance
Steam LinesPressure TightPressure Tight
TanksCorrosion ResistanceCorrosion Resistance
Water LinesBrazing CharacteristicsBrazability
Water LinesCorrosion ResistanceCorrosion Resistance
Water LinesForming CharacteristicsFormability
Water LinesSolderabilitySolderability
PlumbingPlumbing FittingsCorrosion ResistanceCorrosion Resistance
Plumbing FittingsCorrosion ResistanceCorrosion Resistance to Hydrogen Embrittlement
Plumbing FittingsForming CharacteristicsFormability
Plumbing FittingsSolderabilitySolderability
Applicable Specifications
Form Specific Sub-Form Temper Application System Standard Description
ASTMB224Standard Classification of Coppers
ASTMB577Detection of Cuperous Oxide (Hydrogen Embrittlement Susceptibility) in Copper
BandsProjectile RotatingMILITARYMIL-B-20292BLANKS, ROTATING BAND, FOR PROJECTILES
Brazing Filler MetalFEDERALQQ-B-650BRAZING ALLOY, COPPER, COPPER-ZINC, AND COPPER-PHOSPHORUS
Bus Bar, Rod and Shapes, General Purpose, same ASMESB187COPPER BUS BAR, ROD AND SHAPES AND GENERAL PURPOSE ROD, BAR AND SHAPES
ASTMB187/B187MCOPPER BUS BAR, ROD AND SHAPES AND GENERAL PURPOSE ROD, BAR AND SHAPES
Condenser & Heat Exchanger Tube with Integral FinsASMESB359COPPER & COPPER ALLOY SEAMLESS CONDENSER & HEAT EXCHANGER TUBES WITH INTEGRAL FINS
PipeASTMB42SEAMLESS COPPER PIPE, STANDARD SIZES
ASTMB698COPPER, COPPER ALLOY PLUMBING PIPE AND TUBE
Pipe, Seamless. Standard SizesASMESB42SEAMLESS COPPER PIPE, STANDARD SIZES
PlateCladASTMB432COPPER AND COPPER ALLOY CLAD STEEL PLATE
Refinery ShapesASTMB379PHOSPHORIZED COPPERS-REFINERY SHAPES
Seamless Condenser Tube & Ferrule StockASMESB111COPPER AND COPPER ALLOY SEAMLESS CONDENSER TUBES & FERRULE STOCK
Condenser TubeASTMB111/B111MCOPPER AND COPPER ALLOY SEAMLESS CONDENSER TUBES AND FERRULE STOCK
Seamless TubeASMESB75SEAMLESS COPPER TUBE
Sheet, Strip, Roller Bar & PlateASMESB152COPPER SHEET, STRIP, PLATE, AND ROLLED BAR
ASTMB152/B152MCOPPER SHEET, STRIP, PLATE AND ROLLED BAR
StripASTMB272COPPER FLAT PRODUCTS WITH FINISHED (ROLLED OR DRAWN) EDGES (FLAT WIRE AND STRIP)
TubeFinnedASTMB359/B359MCOPPER AND COPPER-ALLOY SEAMLESS CONDENSER AND HEAT EXCHANGER TUBES WITH INTEGRAL FINS
CapillaryASTMB360HARD-DRAWN COPPER CAPILLARY TUBE FOR RESTRICTOR APPLICATIONS
U-BendASTMB395/B395MU-BEND SEAMLESS COPPER AND COPPER ALLOY HEAT EXCHANGER AND CONDENSER TUBES
WeldedASTMB447WELDED COPPER TUBE
WeldedASTMB543/B543MWELDED COPPER AND COPPER ALLOY HEAT EXCHANGER TUBE
WeldedASTMB641SEAMLESS AND WELDED COPPER DISTRIBUTION TUBE (TYPE D)
SeamlessASTMB641SEAMLESS AND WELDED COPPER DISTRIBUTION TUBE (TYPE D)
SeamlessAnnealed Tempers, OBright AnnealedASTMB68/B68MSEAMLESS COPPER TUBE, BRIGHT ANNEALED
ASTMB698COPPER, COPPER ALLOY PLUMBING PIPE AND TUBE
WeldedASTMB716WELDED COPPER WATER TUBE
ASTMB743SEAMLESS COPPER TUBE IN COILS
SeamlessASTMB75/B75MSEAMLESS COPPER TUBE
SeamlessMILITARYMIL-T-24107TUBE, COPPER, SEAMLESS
Tube, Welded Heater ExchangerASMESB543WELDED COPPER AND COPPER ALLOY TUBE
Tubes, Seamless Condenser & Heat Exchanger, U-BendASMESB395U-BEND SEAMLESS COPPER & COPPER ALLOY HEAT EXCHANGER & CONDENSER TUBE
WireFlatASTMB272COPPER FLAT PRODUCTS WITH FINISHED (ROLLED OR DRAWN) EDGES (FLAT WIRE AND STRIP)