Find suppliers for this alloy
C10850
| Elements | |||
|---|---|---|---|
| Cu(1,2) | Mg | O | |
|
(1) Cu + Sum of Named Elements, 99.95% min. (2) This is a high conductivity copper which has, in the annealed condition a minimum conductivity of 100% IACS. |
|||
| Min (%) | 99.95 | 0.002 | |
| Max (%) | 0.013 | 0.001 | |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Vickers Hardness, 3000 gm |
|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||
| Sheet | 1/4 Hard | H01 |
35 Min 38 Typ 46 Max |
37 Typ |
23 Typ |
92 Typ |
| 1/2 Hard | H02 |
40 Min 44 Typ 50 Max |
44 Typ |
13 Typ |
102 Typ |
|
| Extra Hard | H06 |
46 Min 52 Typ 60 Max |
51 Typ |
4 Typ |
113 Typ |
|
| Extra Spring | H10 |
51 Min 58 Typ 66 Max |
56 Typ |
4 Typ |
123 Typ |
|
| 1/8 Hard | H00 |
31 Min 35 Typ 40 Max |
23 Typ |
43 Typ |
72 Typ |
|
| Strip | 1/4 Hard | H01 |
35 Min 38 Typ 46 Max |
37 Typ |
23 Typ |
92 Typ |
| 1/2 Hard | H02 |
40 Min 44 Typ 50 Max |
44 Typ |
13 Typ |
102 Typ |
|
| Extra Hard | H06 |
46 Min 52 Typ 60 Max |
51 Typ |
4 Typ |
113 Typ |
|
| Extra Spring | H10 |
51 Min 58 Typ 66 Max |
56 Typ |
4 Typ |
123 Typ |
|
| 1/8 Hard | H00 |
31 Min 35 Typ 40 Max |
23 Typ |
43 Typ |
72 Typ |
|
| Melting Point - Liquidus°F | 1985 |
|---|---|
| Melting Point - Solidus°F | 1985 |
| Densitylb/cu in. at 68°F | 0.323 |
| Specific Gravity | 8.94 |
| Electrical Conductivity% IACS at 68°F | 101 |
| Electrical Resistivityohm.cmil/ft at 68°F | 10.3 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 226 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.8 |
| Modulus of Elasticity in Tensionksi | 17110 |
| Poisson's Ratioksi | 0.31 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Spot Weld | Excellent |
| Butt Weld | Excellent |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Excellent |
Common Fabrication Processes
- Forming and Bending
- Blanking
- Coining
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Electrical | Electrical Connectors | Conductivity (Electrical) | High Strength & Conductivity |
| Terminals | Conductivity (Electrical) | High Strength & Conductivity | |
| Connectors, Electrical, Lead-Free | |||
| Busbars | Conductivity (Electrical) | Electrical Conductivity | |
| Lead Frames | Conductivity (Electrical) | Electrical Conductivity |
Applicable Specifications