Find suppliers for this alloy
C10910
| Elements | ||
|---|---|---|
| Cu(1,2) | O | |
|
(1) This is a high conductivity copper which has, in the annealed condition a minimum conductivity of 100% IACS. (2) Cu value includes Ag. |
||
| Min (%) | 99.95 | |
| Max (%) | 0.005 | |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Rockwell F scale | Rockwell 30T scale | Shear Strength (ksi) |
Fatigue Strength** (ksi) |
Section Size (in) |
|---|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | |||||||||||
| Flat Products | 1/2 Hard | H02 |
42 Typ |
36 Typ |
14 Typ |
40 Typ |
84 Typ |
50 Typ |
26 Typ |
13 Typ | 0.04 |
| 1/4 Hard | H01 |
38 Typ |
30 Typ |
35 Typ |
25 Typ |
70 Typ |
64 Typ |
25 Typ |
11 Typ | 0.25 | |
| 1/4 Hard | H01 |
38 Typ |
30 Typ |
25 Typ |
25 Typ |
70 Typ |
36 Typ |
25 Typ |
0.04 | ||
| 1/8 Hard | H00 |
36 Typ |
28 Typ |
40 Typ |
10 Typ |
60 Typ |
64 Typ |
25 Typ |
11 Typ | 0.25 | |
| 1/8 Hard | H00 |
36 Typ |
28 Typ |
30 Typ |
10 Typ |
60 Typ |
25 Typ |
25 Typ |
0.04 | ||
| As Hot Rolled | M20 |
32 Typ |
10 Typ |
50 Typ |
50 Typ |
40 Typ |
64 Typ |
22 Typ |
11 Typ | 0.25 | |
| As Hot Rolled | M20 |
34 Typ |
10 Typ |
45 Typ |
62 Typ |
45 Typ |
64 Typ |
23 Typ |
14 Typ | 0.04 | |
| Extra Spring | H10 |
57 Typ |
53 Typ |
4 Typ |
62 Typ |
95 Typ |
64 Typ |
29 Typ |
14 Typ | 0.04 | |
| Hard | H04 |
50 Typ |
45 Typ |
12 Typ |
50 Typ |
90 Typ |
64 Typ |
28 Typ |
11 Typ | 0.25 | |
| Hard | H04 |
45 Typ |
40 Typ |
20 Typ |
45 Typ |
85 Typ |
64 Typ |
26 Typ |
11 Typ | 1 | |
| Hard | H04 |
50 Typ |
45 Typ |
6 Typ |
50 Typ |
90 Typ |
57 Typ |
28 Typ |
13 Typ | 0.04 | |
| Nominal Grain Size 0.025 mm | OS025 |
34 Typ |
11 Typ |
45 Typ |
62 Typ |
45 Typ |
64 Typ |
23 Typ |
11 Typ | 0.04 | |
| Nominal Grain Size 0.050 mm | OS050 |
32 Typ |
10 Typ |
45 Typ |
62 Typ |
40 Typ |
64 Typ |
22 Typ |
11 Typ | 0.04 | |
| Nominal Grain Size 0.050 mm | OS050 |
32 Typ |
10 Typ |
50 Typ |
50 Typ |
40 Typ |
64 Typ |
22 Typ |
11 Typ | 0.25 | |
| Spring | H08 |
55 Typ |
50 Typ |
4 Typ |
60 Typ |
94 Typ |
63 Typ |
29 Typ |
14 Typ | 0.04 | |
| Melting Point - Liquidus°F | 1981 |
|---|---|
| Melting Point - Solidus°F | 1981 |
| Densitylb/cu in. at 68°F | 0.323 |
| Specific Gravity | 8.94 |
| Electrical Conductivity% IACS at 68°F | 100 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 226 |
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 9.4 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 9.6 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.8 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.092 |
| Modulus of Elasticity in Tensionksi | 17000 |
| Modulus of Rigidityksi | 6400 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Fair |
| Gas Shielded Arc Welding | Good |
| Coated Metal Arc Welding | Not Recommended |
| Spot Weld | Not Recommended |
| Butt Weld | Good |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Excellent |
| Forgeability Rating | 65 |
| Machinability Rating | 20 |
Common Fabrication Processes
- Blanking
- Coining
- Coppersmithing
- Drawing
- Etching
- Forming and Bending
- Heading and Upsetting
- Hot Forming
- Piercing and Punching
- Roll Threading and Knurling
- Shearing
- Spinning
- Squeezing and Swaging
- Stamping
| Treatment | Minimum* | Value* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Stress Relief | 356 | |||
| Annealing | 662 | |||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Electrical | Busbars | Brazing Characteristics | Brazability |
| Busbars | Conductivity (Electrical) | Electrical Conductivity | |
| Busbars | Conductivity (Thermal) | Thermal Conductivity | |
| Busbars | Corrosion Resistance | Corrosion Resistance | |
| Busbars | Welding Characteristics | Weldability | |
| Conductors, Electrical | Conductivity (Electrical) | Electrical Conductivity | |
| Conductors, Electrical | Conductivity (Thermal) | Thermal Conductivity | |
| Conductors, Electrical | Corrosion Resistance | Corrosion Resistance | |
| Telecommunication Cables | Conductivity (Electrical) | Electrical Conductivity | |
| Welding and Brazing Components | Welding Characteristics | Weldability |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Bar | ASTM | B152/B152M | COPPER SHEET, STRIP, PLATE AND ROLLED BAR | ||
| Sheet, Strip, Roller Bar & Plate | ASME | SB152 | COPPER SHEET, STRIP, PLATE, AND ROLLED BAR | ||
| Strip | ASTM | B152/B152M | COPPER SHEET, STRIP, PLATE AND ROLLED BAR |
Corrosion Properties