Chemical Composition
Element
Cu(1,2)O
(1) This is a high conductivity copper which has, in the annealed condition a minimum conductivity of 100% IACS. (2) Cu value includes Ag.
Min (%)99.95
Max (%)0.005
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell F scale
Rockwell 30T scale
Shear Strength
(ksi)
Fatigue Strength**
(ksi)
Section Size
(in)
Flat Products1/2 HardH0242   Typ
36   Typ
14   Typ
40   Typ
84   Typ
50   Typ
26   Typ
13   Typ
0.04
1/4 HardH0138   Typ
30   Typ
35   Typ
25   Typ
70   Typ
64   Typ
25   Typ
11   Typ
0.25
H0138   Typ
30   Typ
25   Typ
25   Typ
70   Typ
36   Typ
25   Typ
0.04
1/8 HardH0036   Typ
28   Typ
40   Typ
10   Typ
60   Typ
64   Typ
25   Typ
11   Typ
0.25
H0036   Typ
28   Typ
30   Typ
10   Typ
60   Typ
25   Typ
25   Typ
0.04
As Hot RolledM2032   Typ
10   Typ
50   Typ
50   Typ
40   Typ
64   Typ
22   Typ
11   Typ
0.25
M2034   Typ
10   Typ
45   Typ
62   Typ
45   Typ
64   Typ
23   Typ
14   Typ
0.04
Extra SpringH1057   Typ
53   Typ
4   Typ
62   Typ
95   Typ
64   Typ
29   Typ
14   Typ
0.04
HardH0450   Typ
45   Typ
12   Typ
50   Typ
90   Typ
64   Typ
28   Typ
11   Typ
0.25
H0445   Typ
40   Typ
20   Typ
45   Typ
85   Typ
64   Typ
26   Typ
11   Typ
1
H0450   Typ
45   Typ
6   Typ
50   Typ
90   Typ
57   Typ
28   Typ
13   Typ
0.04
Nominal Grain Size 0.025 mmOS02534   Typ
11   Typ
45   Typ
62   Typ
45   Typ
64   Typ
23   Typ
11   Typ
0.04
Nominal Grain Size 0.050 mmOS05032   Typ
10   Typ
45   Typ
62   Typ
40   Typ
64   Typ
22   Typ
11   Typ
0.04
OS05032   Typ
10   Typ
50   Typ
50   Typ
40   Typ
64   Typ
22   Typ
11   Typ
0.25
SpringH0855   Typ
50   Typ
4   Typ
60   Typ
94   Typ
63   Typ
29   Typ
14   Typ
0.04
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
Melting Point - Liquidus°F1981
Melting Point - Solidus°F1981
Densitylb/cu in. at 68°F0.323
Specific Gravity8.94
Electrical Conductivity% IACS at 68°F100
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F226
Coefficient of Thermal Expansion 68-21210⁻⁶ per °F (68 – 212°F)9.4
Coefficient of Thermal Expansion 68-39210⁻⁶ per °F (68 – 392°F)9.6
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)9.8
Specific Heat CapacityBtu/ lb /°F at 68°F0.092
Modulus of Elasticity in Tensionksi17000
Modulus of Rigidityksi6400
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingFair
Gas Shielded Arc WeldingGood
Coated Metal Arc WeldingNot Recommended
Spot WeldNot Recommended
Butt WeldGood
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedExcellent
Forgeability Rating65
Machinability Rating20
Common Fabrication Processes
  • Blanking
  • Coining
  • Coppersmithing
  • Drawing
  • Etching
  • Forming and Bending
  • Heading and Upsetting
  • Hot Forming
  • Piercing and Punching
  • Roll Threading and Knurling
  • Shearing
  • Spinning
  • Squeezing and Swaging
  • Stamping
    
Thermal Properties
Treatment Minimum* Value*
* Temperature is measured in Fahrenheit.
Stress Relief356
Annealing662
Typical uses
Product Category Product Reason Category Reason
ElectricalBusbarsBrazing CharacteristicsBrazability
BusbarsConductivity (Electrical)Electrical Conductivity
BusbarsConductivity (Thermal)Thermal Conductivity
BusbarsCorrosion ResistanceCorrosion Resistance
BusbarsWelding CharacteristicsWeldability
Conductors, ElectricalConductivity (Electrical)Electrical Conductivity
Conductors, ElectricalConductivity (Thermal)Thermal Conductivity
Conductors, ElectricalCorrosion ResistanceCorrosion Resistance
Telecommunication CablesConductivity (Electrical)Electrical Conductivity
Welding and Brazing ComponentsWelding CharacteristicsWeldability
Applicable Specifications
Form System Standard Description
BarASTMB152/B152MCOPPER SHEET, STRIP, PLATE AND ROLLED BAR
Sheet, Strip, Roller Bar & PlateASMESB152COPPER SHEET, STRIP, PLATE, AND ROLLED BAR
StripASTMB152/B152MCOPPER SHEET, STRIP, PLATE AND ROLLED BAR
Corrosion Properties