| Elements | ||
|---|---|---|
| Cu(1) | P | |
|
(1) Cu value includes Ag. |
||
| Min (%) | 99.90 | 0.015 |
| Max (%) | 0.025 | |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Rockwell F scale | Rockwell 30T scale | Shear Strength (ksi) |
Fatigue Strength** (ksi) |
Section Size (in) |
Cold Work (%) |
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | ||||||||||||
| Flat Products | 1/2 Hard | H02 |
42 Typ |
36 Typ |
14 Typ |
40 Typ |
84 Typ |
50 Typ |
26 Typ |
13 Typ | 0.04 | |
| 1/4 Hard | H01 |
38 Typ |
30 Typ |
25 Typ |
25 Typ |
70 Typ |
36 Typ |
25 Typ |
0.04 | |||
| 1/4 Hard | H01 |
38 Typ |
30 Typ |
35 Typ |
25 Typ |
70 Typ |
25 Typ |
0.25 | ||||
| 1/8 Hard | H00 |
36 Typ |
28 Typ |
40 Typ |
10 Typ |
60 Typ |
25 Typ |
0.25 | ||||
| 1/8 Hard | H00 |
36 Typ |
28 Typ |
30 Typ |
10 Typ |
60 Typ |
25 Typ |
25 Typ |
0.04 | |||
| As Hot Rolled | M20 |
32 Typ |
10 Typ |
50 Typ |
40 Typ |
22 Typ |
0.25 | |||||
| As Hot Rolled | M20 |
34 Typ |
10 Typ |
45 Typ |
45 Typ |
23 Typ |
0.04 | |||||
| Extra Spring | H10 |
57 Typ |
53 Typ |
4 Typ |
62 Typ |
95 Typ |
64 Typ |
29 Typ |
0.04 | |||
| Hard | H04 |
45 Typ |
40 Typ |
20 Typ |
85 Typ |
26 Typ |
1 | |||||
| Hard | H04 |
50 Typ |
45 Typ |
6 Typ |
50 Typ |
90 Typ |
57 Typ |
28 Typ |
13 Typ | 0.04 | ||
| Hard | H04 |
50 Typ |
45 Typ |
12 Typ |
50 Typ |
90 Typ |
28 Typ |
0.25 | ||||
| Nominal Grain Size 0.025 mm | OS025 |
34 Typ |
11 Typ |
45 Typ |
45 Typ |
23 Typ |
11 Typ | 0.04 | ||||
| Nominal Grain Size 0.050 mm | OS050 |
32 Typ |
10 Typ |
45 Typ |
40 Typ |
22 Typ |
0.04 | |||||
| Nominal Grain Size 0.050 mm | OS050 |
32 Typ |
10 Typ |
50 Typ |
40 Typ |
22 Typ |
0.25 | |||||
| Spring | H08 |
55 Typ |
50 Typ |
4 Typ |
60 Typ |
94 Typ |
63 Typ |
29 Typ |
14 Typ | 0.04 | ||
| Pipe | Hard | H04 |
50 Typ |
45 Typ |
10 Typ |
50 Typ |
90 Typ |
28 Typ |
30 | |||
| Tube | Hard Drawn | H80 |
55 Typ |
50 Typ |
8 Typ |
60 Typ |
95 Typ |
63 Typ |
29 Typ |
19 Typ | 0.065 | 40 |
| Light Drawn, Light Cold Rolled | H55 |
40 Typ |
32 Typ |
25 Typ |
35 Typ |
77 Typ |
45 Typ |
26 Typ |
14 Typ | 0.065 | 15 | |
| Nominal Grain Size 0.025 mm | OS025 |
34 Typ |
11 Typ |
45 Typ |
45 Typ |
23 Typ |
0.065 | |||||
| Nominal Grain Size 0.050 mm | OS050 |
32 Typ |
10 Typ |
45 Typ |
40 Typ |
22 Typ |
11 Typ | 0.065 | ||||
| Melting Point - Liquidus°F | 1981 |
|---|---|
| Densitylb/cu in. at 68°F | 0.323 |
| Specific Gravity | 8.94 |
| Electrical Conductivity% IACS at 68°F | 85 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 196 |
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 9.4 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 9.5 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.8 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.092 |
| Modulus of Elasticity in Tensionksi | 17000 |
| Modulus of Rigidityksi | 6400 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Good |
| Gas Shielded Arc Welding | Excellent |
| Coated Metal Arc Welding | Not Recommended |
| Spot Weld | Not Recommended |
| Seam Weld | Not Recommended |
| Butt Weld | Good |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Excellent |
| Forgeability Rating | 65 |
| Machinability Rating | 20 |
Common Fabrication Processes
- Blanking
- Coining
- Coppersmithing
- Drawing
- Etching
- Forming and Bending
- Heading and Upsetting
- Hot Forging and Pressing
- Piercing and Punching
- Roll Threading and Knurling
- Shearing
- Spinning
- Squeezing and Swaging
- Stamping
Thermal Properties
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Automotive | Air Lines | Corrosion Resistance | Corrosion Resistance |
| Air Lines | Pressure Tight | Pressure Tight | |
| Air Lines | Solderability | Solderability | |
| Air Lines | Welding Characteristics | Weldability | |
| Gasoline Lines | Corrosion Resistance | Corrosion Resistance | |
| Gasoline Lines | Forming Characteristics | Formability | |
| Gasoline Lines | Pressure Tight | Pressure Tight | |
| Gasoline Lines | Solderability | Solderability | |
| Hydraulic Lines | Corrosion Resistance | Corrosion Resistance | |
| Hydraulic Lines | Pressure Tight | Pressure Tight | |
| Hydraulic Lines | Solderability | Solderability | |
| Hydraulic Lines | Welding Characteristics | Weldability | |
| Oil Lines | Forming Characteristics | Formability | |
| Oil Lines | Mechanical Properties | Strength | |
| Building | Air Conditioner Tubes and Condenser Sheets | Conductivity (Thermal) | Thermal Conductivity |
| Air Conditioner Tubes and Condenser Sheets | Corrosion Resistance | Corrosion Resistance | |
| Air Conditioner Tubes and Condenser Sheets | Mechanical Properties | Moderate Strength | |
| Gas Lines | Corrosion Resistance | Corrosion Resistance | |
| Gas Lines | Forming Characteristics | Formability | |
| Gas Lines | Pressure Tight | Pressure Tight | |
| Gas Lines | Solderability | Solderability | |
| Gas Lines | Welding Characteristics | Weldability | |
| Heater Lines | Conductivity (Thermal) | Thermal Conductivity | |
| Heater Lines | Corrosion Resistance | Corrosion Resistance | |
| Heater Lines | Pressure Tight | Pressure Tight | |
| Heater Lines | Welding Characteristics | Weldability | |
| Heater Units | Conductivity (Thermal) | Thermal Conductivity | |
| Heater Units | Corrosion Resistance | Corrosion Resistance | |
| Heater Units | Welding Characteristics | Weldability | |
| Oil Burner Tubes | Corrosion Resistance | Corrosion Resistance | |
| Oil Burner Tubes | Pressure Tight | Pressure Tight | |
| Oil Burner Tubes | Solderability | Solderability | |
| Oil Burner Tubes | Welding Characteristics | Weldability | |
| Consumer | Air Conditioners | Brazing Characteristics | Brazability |
| Air Conditioners | Corrosion Resistance | Corrosion Resistance | |
| Air Conditioners | Pressure Tight | Pressure Tight | |
| Refrigerators | Conductivity (Thermal) | Thermal Conductivity | |
| Refrigerators | Corrosion Resistance | Corrosion Resistance | |
| Refrigerators | Forming Characteristics | Formability | |
| Refrigerators | Pressure Tight | Pressure Tight | |
| Industrial | Air Lines in Airplanes | Corrosion Resistance | Corrosion Resistance |
| Air Lines in Airplanes | Pressure Tight | Pressure Tight | |
| Air Lines in Airplanes | Solderability | Solderability | |
| Brewery Tubes | Corrosion Resistance | Corrosion Resistance | |
| Brewery Tubes | Solderability | Solderability | |
| Brewery Tubes | Welding Characteristics | Weldability | |
| Casting Molds | Conductivity (Thermal) | Thermal Conductivity | |
| Casting Molds | Corrosion Resistance | Corrosion Resistance | |
| Casting Molds | Friction & Wear Properties | Wear Resistance | |
| Casting Molds | Mechanical Properties | Moderate Strength | |
| Condenser Tubes | Conductivity (Thermal) | Thermal Conductivity | |
| Condenser Tubes | Corrosion Resistance | Corrosion Resistance | |
| Condenser Tubes | Pressure Tight | Pressure Tight | |
| Dairy Tubes | Conductivity (Thermal) | Thermal Conductivity | |
| Dairy Tubes | Corrosion Resistance | Corrosion Resistance | |
| Dairy Tubes | Pressure Tight | Pressure Tight | |
| Dairy Tubes | Solderability | Solderability | |
| Dairy Tubes | Welding Characteristics | Weldability | |
| Distiller Tubes | Conductivity (Thermal) | Thermal Conductivity | |
| Distiller Tubes | Corrosion Resistance | Corrosion Resistance | |
| Distiller Tubes | Welding Characteristics | Weldability | |
| Evaporator Tubes | Conductivity (Thermal) | Thermal Conductivity | |
| Evaporator Tubes | Corrosion Resistance | Corrosion Resistance | |
| Evaporator Tubes | Pressure Tight | Pressure Tight | |
| Evaporator Tubes | Welding Characteristics | Weldability | |
| Gage Lines | Conductivity (Thermal) | Thermal Conductivity | |
| Gage Lines | Corrosion Resistance | Corrosion Resistance | |
| Gage Lines | Pressure Tight | Pressure Tight | |
| Gage Lines | Solderability | Solderability | |
| Gage Lines | Welding Characteristics | Weldability | |
| Gasoline Lines in Airplanes | Corrosion Resistance | Corrosion Resistance | |
| Gasoline Lines in Airplanes | Forming Characteristics | Formability | |
| Gasoline Lines in Airplanes | Pressure Tight | Pressure Tight | |
| Gasoline Lines in Airplanes | Welding Characteristics | Weldability | |
| Heat Exchanger Tubes | Conductivity (Thermal) | Thermal Conductivity | |
| Heat Exchanger Tubes | Corrosion Resistance | Corrosion Resistance | |
| Heat Exchanger Tubes | Pressure Tight | Pressure Tight | |
| Heat Exchanger Tubes | Welding Characteristics | Weldability | |
| Hydraulic Lines in Airplanes | Corrosion Resistance | Corrosion Resistance | |
| Hydraulic Lines in Airplanes | Pressure Tight | Pressure Tight | |
| Hydraulic Lines in Airplanes | Welding Characteristics | Weldability | |
| Kettles | Appearance | Appearance | |
| Kettles | Conductivity (Thermal) | Thermal Conductivity | |
| Kettles | Corrosion Resistance | Corrosion Resistance | |
| Oil Coolers in Airplanes | Corrosion Resistance | Corrosion Resistance | |
| Oil Coolers in Airplanes | Pressure Tight | Pressure Tight | |
| Oil Coolers in Airplanes | Solderability | Solderability | |
| Oil Coolers in Airplanes | Welding Characteristics | Weldability | |
| Oil Lines in Airplanes | Corrosion Resistance | Corrosion Resistance | |
| Oil Lines in Airplanes | Pressure Tight | Pressure Tight | |
| Oil Lines in Airplanes | Solderability | Solderability | |
| Oil Lines in Airplanes | Welding Characteristics | Weldability | |
| Paper Lines | Conductivity (Thermal) | Thermal Conductivity | |
| Paper Lines | Corrosion Resistance | Corrosion Resistance | |
| Paper Lines | Welding Characteristics | Weldability | |
| Plating Anodes | Conductivity (Electrical) | Electrical Conductivity | |
| Plating Anodes | Corrosion Resistance | Corrosion Resistance to Chemicals | |
| Plating Anodes | Plating Characteristics | Platability | |
| Plating Hangers | Conductivity (Electrical) | Electrical Conductivity | |
| Plating Hangers | Corrosion Resistance | Corrosion Resistance | |
| Plating Hangers | Corrosion Resistance | Corrosion Resistance to Chemicals | |
| Plating Racks | Conductivity (Electrical) | Electrical Conductivity | |
| Plating Racks | Corrosion Resistance | Corrosion Resistance to Chemicals | |
| Plating Racks | Plating Characteristics | Plateable | |
| Plumbing Tube | Conductivity (Electrical) | Electrical Conductivity | |
| Plumbing Tube | Corrosion Resistance | Corrosion Resistance | |
| Plumbing Tube | Forming Characteristics | Formability | |
| Plumbing Tube | Welding Characteristics | Weldability | |
| Pulp Lines | Conductivity (Thermal) | Thermal Conductivity | |
| Pulp Lines | Corrosion Resistance | Corrosion Resistance | |
| Pulp Lines | Welding Characteristics | Weldability | |
| Rotating Bands | Conductivity (Thermal) | Thermal Conductivity | |
| Rotating Bands | Corrosion Resistance | Corrosion Resistance | |
| Steam Lines | Conductivity (Thermal) | Thermal Conductivity | |
| Steam Lines | Corrosion Resistance | Corrosion Resistance | |
| Steam Lines | Creep Properties | Creep Resistant | |
| Steam Lines | Pressure Tight | Pressure Tight | |
| Steam Lines | Softening Resistance | Resistance to Thermal Softening | |
| Steam Lines | Welding Characteristics | Weldability | |
| Tanks | Corrosion Resistance | Corrosion Resistance | |
| Water Lines | Corrosion Resistance | Corrosion Resistance | |
| Water Lines | Solderability | Solderability | |
| Water Lines | Welding Characteristics | Weldability | |
| Marine | Oil Coolers | Corrosion Resistance | Corrosion Resistance |
| Oil Coolers | Solderability | Solderability | |
| Oil Coolers | Welding Characteristics | Weldability | |
| Oil Lines | Corrosion Resistance | Corrosion Resistance | |
| Oil Lines | Pressure Tight | Pressure Tight | |
| Oil Lines | Solderability | Solderability | |
| Oil Lines | Welding Characteristics | Weldability | |
| Plumbing | Plumbing Fittings | Corrosion Resistance | Corrosion Resistance |
| Plumbing Fittings | Corrosion Resistance | Corrosion Resistance to Hydrogen Embrittlememt | |
| Plumbing Fittings | Solderability | Solderability | |
| Plumbing Pipe | Corrosion Resistance | Corrosion Resistance | |
| Plumbing Pipe | Forming Characteristics | Formability | |
| Plumbing Pipe | Solderability | Solderability |
Applicable Specifications