Find suppliers for this alloy
C14200
| Elements | |||
|---|---|---|---|
| Cu(1) | P | As | |
|
(1) Cu value includes Ag. |
|||
| Min (%) | 99.4 | 0.015 | 0.15 |
| Max (%) | 0.040 | 0.50 | |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Rockwell F scale | Rockwell 30T scale | Shear Strength (ksi) |
Fatigue Strength** (ksi) |
Section Size (in) |
Cold Work (%) |
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | ||||||||||||
| Flat Products | Nominal Grain Size 0.050 mm | OS050 |
32 Typ |
10 Typ |
45 Typ |
40 Typ |
22 Typ |
0.04 | ||||
| Pipe | Hard | H04 |
50 Typ |
45 Typ |
10 Typ |
50 Typ |
90 Typ |
28 Typ |
30 | |||
| Tube | Hard Drawn | H80 |
55 Typ |
50 Typ |
8 Typ |
60 Typ |
95 Typ |
63 Typ |
29 Typ |
19 Typ | 0.065 | 40 |
| Light Drawn, Light Cold Rolled | H55 |
40 Typ |
32 Typ |
25 Typ |
35 Typ |
77 Typ |
45 Typ |
26 Typ |
14 Typ | 0.065 | 15 | |
| Nominal Grain Size 0.025 mm | OS025 |
34 Typ |
11 Typ |
45 Typ |
45 Typ |
23 Typ |
0.065 | |||||
| Nominal Grain Size 0.050 mm | OS050 |
32 Typ |
10 Typ |
45 Typ |
40 Typ |
22 Typ |
11 Typ | 0.065 | ||||
| Melting Point - Liquidus°F | 1978 |
|---|---|
| Densitylb/cu in. at 68°F | 0.323 |
| Specific Gravity | 8.91 |
| Electrical Conductivity% IACS at 68°F | 45 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 112 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.8 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.092 |
| Modulus of Elasticity in Tensionksi | 17000 |
| Modulus of Rigidityksi | 6400 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Good |
| Coated Metal Arc Welding | Not Recommended |
| Spot Weld | Not Recommended |
| Seam Weld | Not Recommended |
| Butt Weld | Good |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Excellent |
| Forgeability Rating | 65 |
| Machinability Rating | 20 |
Common Fabrication Processes
- Drawing
- Forming and Bending
- Heading and Upsetting
- Piercing and Punching
- Roll Threading and Knurling
- Shearing
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 800 | 1200 | ||
| Hot Working Temperature | 1400 | 1600 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Industrial | Condenser Tubes | Conductivity (Thermal) | Thermal Conductivity |
| Condenser Tubes | Corrosion Resistance | Corrosion Resistance | |
| Condenser Tubes | Mechanical Properties | Creep Resistance | |
| Condenser Tubes | Softening Resistance | Resistance to Thermal Softening | |
| Condenser Tubes | Solderability | Solderability | |
| Condenser Tubes | Welding Characteristics | Weldability | |
| Heat Exchanger Tubes | Conductivity (Thermal) | Thermal Conductivity | |
| Heat Exchanger Tubes | Corrosion Resistance | Corrosion Resistance | |
| Heat Exchanger Tubes | Mechanical Properties | Creep Resistance | |
| Heat Exchanger Tubes | Softening Resistance | Resistance to Thermal Softening | |
| Heat Exchanger Tubes | Solderability | Solderability | |
| Heat Exchanger Tubes | Welding Characteristics | Weldability | |
| Plates for Locomotive Fire boxes | Conductivity (Thermal) | Thermal Conductivity | |
| Plates for Locomotive Fire boxes | Corrosion Resistance | Corrosion Resistance | |
| Plates for Locomotive Fire boxes | Mechanical Properties | Creep Resistance | |
| Plates for Locomotive Fire boxes | Softening Resistance | Resistance to Thermal Softening | |
| Plates for Locomotive Fire boxes | Solderability | Solderability | |
| Plumbing Tube | Conductivity (Thermal) | Thermal Conductivity | |
| Plumbing Tube | Corrosion Resistance | Corrosion Resistance | |
| Plumbing Tube | Mechanical Properties | Strength | |
| Plumbing Tube | Softening Resistance | Resistance to Softening | |
| Stay bolts | Conductivity (Thermal) | Thermal Conductivity | |
| Stay bolts | Corrosion Resistance | Corrosion Resistance | |
| Stay bolts | Mechanical Properties | Creep Resistance | |
| Stay bolts | Softening Resistance | Resistance to Thermal Softening | |
| Other | Locomotive Steam Boiler | Conductivity (Thermal) | Thermal Conductivity |
| Locomotive Steam Boiler | Corrosion Resistance | Corrosion Resistance | |
| Locomotive Steam Boiler | Mechanical Properties | Strength | |
| Locomotive Steam Boiler | Softening Resistance | Resistance to Softening |
Applicable Specifications
Corrosion Properties