Find suppliers for this alloyCopper Alloy C14200
Chemical Composition
Element
Cu(1)PAs
(1) Cu value includes Ag.
Min (%)99.40.0150.15
Max (%)0.0400.50
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell F scale
Rockwell 30T scale
Shear Strength
(ksi)
Fatigue Strength**
(ksi)
Section Size
(in)
Cold Work
(%)
Flat ProductsNominal Grain Size 0.050 mmOS05032   Typ
10   Typ
45   Typ
40   Typ
22   Typ
0.04
PipeHardH0450   Typ
45   Typ
10   Typ
50   Typ
90   Typ
28   Typ
30
TubeHard DrawnH8055   Typ
50   Typ
8   Typ
60   Typ
95   Typ
63   Typ
29   Typ
19   Typ
0.06540
Light Drawn, Light Cold RolledH5540   Typ
32   Typ
25   Typ
35   Typ
77   Typ
45   Typ
26   Typ
14   Typ
0.06515
Nominal Grain Size 0.025 mmOS02534   Typ
11   Typ
45   Typ
45   Typ
23   Typ
0.065
Nominal Grain Size 0.050 mmOS05032   Typ
10   Typ
45   Typ
40   Typ
22   Typ
11   Typ
0.065
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
Melting Point - Liquidus°F1978
Densitylb/cu in. at 68°F0.323
Specific Gravity8.91
Electrical Conductivity% IACS at 68°F45
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F112
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)9.8
Specific Heat CapacityBtu/ lb /°F at 68°F0.092
Modulus of Elasticity in Tensionksi17000
Modulus of Rigidityksi6400
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingGood
Coated Metal Arc WeldingNot Recommended
Spot WeldNot Recommended
Seam WeldNot Recommended
Butt WeldGood
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedExcellent
Forgeability Rating65
Machinability Rating20
Common Fabrication Processes
  • Drawing
  • Forming and Bending
  • Heading and Upsetting
  • Piercing and Punching
  • Roll Threading and Knurling
  • Shearing
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing8001200
Hot Treatment14001600
    
Typical uses
Product Category Product Reason Category Reason
IndustrialCondenser TubesConductivity (Thermal)Thermal Conductivity
Condenser TubesCorrosion ResistanceCorrosion Resistance
Condenser TubesMechanical PropertiesCreep Resistance
Condenser TubesSoftening ResistanceResistance to Thermal Softening
Condenser TubesSolderabilitySolderability
Condenser TubesWelding CharacteristicsWeldability
Heat Exchanger TubesConductivity (Thermal)Thermal Conductivity
Heat Exchanger TubesCorrosion ResistanceCorrosion Resistance
Heat Exchanger TubesMechanical PropertiesCreep Resistance
Heat Exchanger TubesSoftening ResistanceResistance to Thermal Softening
Heat Exchanger TubesSolderabilitySolderability
Heat Exchanger TubesWelding CharacteristicsWeldability
Plates for Locomotive Fire boxesConductivity (Thermal)Thermal Conductivity
Plates for Locomotive Fire boxesCorrosion ResistanceCorrosion Resistance
Plates for Locomotive Fire boxesMechanical PropertiesCreep Resistance
Plates for Locomotive Fire boxesSoftening ResistanceResistance to Thermal Softening
Plates for Locomotive Fire boxesSolderabilitySolderability
Plumbing TubeConductivity (Thermal)Thermal Conductivity
Plumbing TubeCorrosion ResistanceCorrosion Resistance
Plumbing TubeMechanical PropertiesStrength
Plumbing TubeSoftening ResistanceResistance to Softening
Stay boltsConductivity (Thermal)Thermal Conductivity
Stay boltsCorrosion ResistanceCorrosion Resistance
Stay boltsMechanical PropertiesCreep Resistance
Stay boltsSoftening ResistanceResistance to Thermal Softening
OtherLocomotive Steam BoilerConductivity (Thermal)Thermal Conductivity
Locomotive Steam BoilerCorrosion ResistanceCorrosion Resistance
Locomotive Steam BoilerMechanical PropertiesStrength
Locomotive Steam BoilerSoftening ResistanceResistance to Softening
Applicable Specifications
Form Sub-Form Specific Sub-Form Application System Standard Description
ASTMB577Detection of Cuperous Oxide (Hydrogen Embrittlement Susceptibility) in Copper
BarASTMB152/B152MCOPPER SHEET, STRIP, PLATE AND ROLLED BAR
PlateASTMB152/B152MCOPPER SHEET, STRIP, PLATE AND ROLLED BAR
Refinery ShapesASTMB379PHOSPHORIZED COPPERS-REFINERY SHAPES
Seamless Condenser Tube & Ferrule StockASMESB152COPPER SHEET, STRIP, PLATE, AND ROLLED BAR
Seamless Heat Exchanger and Condenser Tubewith Integral FinsFinnedASMESB359COPPER & COPPER ALLOY SEAMLESS CONDENSER & HEAT EXCHANGER TUBES WITH INTEGRAL FINS
U-BendASMESB395U-BEND SEAMLESS COPPER & COPPER ALLOY HEAT EXCHANGER & CONDENSER TUBE
ShapesASTMB216REFINERY SHAPES, TOUGH-PITCH FIRE-REFINED
SheetASTMB152/B152MCOPPER SHEET, STRIP, PLATE AND ROLLED BAR
StripASTMB152/B152MCOPPER SHEET, STRIP, PLATE AND ROLLED BAR
ASTMB272COPPER FLAT PRODUCTS WITH FINISHED (ROLLED OR DRAWN) EDGES (FLAT WIRE AND STRIP)
TubeCondenser TubeASMESB111COPPER AND COPPER ALLOY SEAMLESS CONDENSER TUBES & FERRULE STOCK
Condenser TubeASTMB111/B111MCOPPER AND COPPER ALLOY SEAMLESS CONDENSER TUBES AND FERRULE STOCK
FinnedASTMB359/B359MCOPPER AND COPPER-ALLOY SEAMLESS CONDENSER AND HEAT EXCHANGER TUBES WITH INTEGRAL FINS
U-BendASTMB395/B395MU-BEND SEAMLESS COPPER AND COPPER ALLOY HEAT EXCHANGER AND CONDENSER TUBES
WeldedASTMB447WELDED COPPER TUBE
SeamlessMILITARYMIL-T-24107TUBE, COPPER, SEAMLESS
Corrosion Properties

No information available.