Find suppliers for this alloyC14300
Chemical Composition
Element
Cu(1,2)Cd
(1) Cu value includes Ag. (2) Includes Cd. Deoxidized with Li or other suitable elements as agreed upon.
Min (%)99.900.05
Max (%)0.15
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.2% Offset
Elongation
(%)
Torsion Modulus
(ksi)
Section Size
(in)
Strip1/2 HardH0245   Typ
40   Typ
14   Typ
0.04
Extra SpringH1058  
56  
3   Typ
6.4   Typ
0.04
H1058   Min
56   Min
1   Typ
0.04
HardH0445   Typ
40   Typ
14   Typ
0.04
H0451   Typ
48   Typ
7   Typ
0.04
Nominal Grain Size 0.025 mmOS02532   Typ
11   Typ
42   Typ
0.04
OS02532   Typ
11   Typ
42   Typ
0.04
SpringH0859   Typ
56   Typ
3   Typ
0.04
H0851   Typ
48   Typ
7   Typ
0.04
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1976
Melting Point - Solidus°F1926
Densitylb/cu in. at 68°F0.323
Specific Gravity8.94
Electrical Conductivity% IACS at 68°F96
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F218
Coefficient of Thermal Expansion 68-21210⁻⁶ per °F (68 – 212°F)9.4
Coefficient of Thermal Expansion 68-39210⁻⁶ per °F (68 – 392°F)9.6
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)9.8
Specific Heat CapacityBtu/ lb /°F at 68°F0.092
Modulus of Elasticity in Tensionksi17000
Modulus of Rigidityksi6400
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingGood
Gas Shielded Arc WeldingExcellent
Coated Metal Arc WeldingNot Recommended
Spot WeldNot Recommended
Seam WeldNot Recommended
Butt WeldGood
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedExcellent
Forgeability Rating65
Machinability Rating20
Common Fabrication Processes
  • Blanking
  • Bonding
  • Deep Drawing
  • Etching
  • Forming
  • Piercing
  • Punching
    
Thermal Properties
Treatment Minimum* Maximum* Value*
* Temperature is measured in Fahrenheit.
Stress Relief750
Annealing10001400
Hot Treatment14001600
Typical uses
Product Category Product Reason Category Reason
AutomotiveFins, Auto RadiatorConductivity (Thermal)Thermal Conductivity
Fins, Auto RadiatorCorrosion ResistanceCorrosion Resistance
Fins, Auto RadiatorMechanical PropertiesModerate Strength
Fins, Auto RadiatorSoftening ResistanceResistance to Softening at Soldering Temperatures
Fins, Auto RadiatorWelding CharacteristicsWeldability
Fins, Heat ExchangerConductivity (Thermal)Thermal Conductivity
Fins, Heat ExchangerCorrosion ResistanceCorrosion Resistance
Fins, Heat ExchangerMechanical PropertiesModerate Strenght
Fins, Heat ExchangerSoftening ResistanceResistance to Softening at Soldering Temperatures
Fins, Heat ExchangerWelding CharacteristicsWeldability
ElectricalCable, Anneal ResistantConductivity (Thermal)Thermal Conductivity
Cable, Anneal ResistantCorrosion ResistanceCorrosion Resistance
Cable, Anneal ResistantMechanical PropertiesCreep Resistance
Cable, Anneal ResistantSoftening ResistanceResistance to Thermal Softening
ContactsConductivity (Electrical)Electrical Conductivity
ContactsConductivity (Thermal)Thermal Conductivity
ContactsCorrosion ResistanceCorrosion Resistance
ContactsMechanical PropertiesCreep Resistance
ContactsSoftening ResistanceResistance to Thermal Softening
ContactsSolderabilitySolderability
Electrical AppliancesConductivity (Electrical)Electrical Conductivity
Electrical AppliancesConductivity (Thermal)Thermal Conductivity
Electrical AppliancesCorrosion ResistanceCorrosion Resistance
Electrical AppliancesMechanical PropertiesCreep Resistance
Electrical AppliancesSoftening ResistanceResistance to Thermal Softening
Lead FramesConductivity (Electrical)Electrical Conductivity
Lead FramesConductivity (Thermal)Thermal Conductivity
Lead FramesCorrosion ResistanceCorrosion Resistance
Lead FramesMechanical PropertiesCreep Resistance
Lead FramesSoftening ResistanceResistance to Thermal Softening
Lead FramesSolderabilitySolderability
Solder Coated PartsCorrosion ResistanceCorrosion Resistance
Solder Coated PartsMechanical PropertiesCreep Resistance
Solder Coated PartsSoftening ResistanceResistance to Thermal Softening
Solder Coated PartsSolderabilitySolderability
Solder Fabricated PartsCorrosion ResistanceCorrosion Resistance
Solder Fabricated PartsMechanical PropertiesCreep Resistance
Solder Fabricated PartsSoftening ResistanceResistance to Thermal Softening
Solder Fabricated PartsSolderabilitySolderability
TerminalsConductivity (Electrical)Electrical Conductivity
TerminalsConductivity (Thermal)Thermal Conductivity
TerminalsCorrosion ResistanceCorrosion Resistance
TerminalsMechanical PropertiesCreep Resistance
TerminalsSoftening ResistanceResistance to Thermal Softening
TerminalsSolderabilitySolderability
IndustrialAir ConditionersConductivity (Thermal)Thermal Conductivity
Air ConditionersCorrosion ResistanceCorrosion Resistance
Air ConditionersPressure TightPressure Tight
Cable WrapConductivity (Thermal)Thermal Conductivity
Cable WrapCorrosion ResistanceCorrosion Resistance
Cable WrapMechanical PropertiesCreep Resistance
Commutators for Small MotorsConductivity (Electrical)Electrical Conductivity
Commutators for Small MotorsConductivity (Thermal)Thermal Conductivity
Commutators for Small MotorsCorrosion ResistanceCorrosion Resistance
Commutators for Small MotorsMechanical PropertiesCreep Resistance
Commutators for Small MotorsSoftening ResistanceResistance to Thermal Softening
Commutators for Small MotorsSolderabilitySolderability
TubeConductivity (Thermal)Thermal Conductivity
TubeCorrosion ResistanceCorrosion Resistance
TubeSolderabilitySolderability
Applicable Specifications
Form System Standard Description
Brazing Filler MetalFEDERALQQ-B-650BRAZING ALLOY, COPPER, COPPER-ZINC, AND COPPER-PHOSPHORUS
Corrosion Properties

No information available.