Find suppliers for this alloy
C14425
| Elements | |||||||
|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Sn | Zn | Fe | P | Ni(3) | |
|
(1) Cu + Sum of Named Elements, 99.97% Min. (2) Cu value includes Ag. (3) Includes Co. |
|||||||
| Min (%) | 99.97 | 0.25 | |||||
| Max (%) | 0.10 | 0.35 | 0.10 | 0.020 | 0.010 | 0.020 | |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
Elongation (%) |
Section Size (in) |
|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||
| Wire | Hard-drawn Electrical Wire | H86 |
116 Typ |
1 Typ |
0.01 |
| Melting Point - Liquidus°F | 1967 |
|---|---|
| Melting Point - Solidus°F | 1949 |
| Densitylb/cu in. at 68°F | 0.321 |
| Specific Gravity | 8.93 |
| Electrical Conductivity% IACS at 68°F | 72 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 169 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 10.1 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 18850 |
| Poisson's Ratio | 0.34 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Good |
| Gas Shielded Arc Welding | Excellent |
| Coated Metal Arc Welding | Not Recommended |
| Spot Weld | Fair |
| Seam Weld | Not Recommended |
| Butt Weld | Poor |
| Machinability Rating | 20 |
Common Fabrication Processes
Thermal Properties
Typical Uses
Applicable Specifications
Corrosion Properties