| Elements | ||||
|---|---|---|---|---|
| Cu(1) | P | O | Te | |
|
(1) Cu + Sum of Named Elements 99.9% min. |
||||
| Min (%) | 99.8 | 0.10 | ||
| Max (%) | 0.003 | 0.001 | 0.50 | |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Vickers Hardness, 3000 gm |
|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||
| Rod & Bar | 1/2 Hard | H02 |
38 Min |
31 Min |
12 Typ |
90 Typ |
| Strip and Sheet | 1/2 Hard | H02 |
38 Min |
31 Min |
12 Typ |
92 Typ |
| Melting Point - Liquidus°F | 1981 |
|---|---|
| Densitylb/cu in. at 68°F | 0.31 |
| Specific Gravity | 7.8 |
| Electrical Conductivity% IACS at 68°F | 95 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 234 |