Chemical Composition
Element
Cu(1,2)PTe
(1) Includes Te + P. (2) Cu value includes Ag.
Min (%)99.900.0040.40
Max (%)0.0200.7
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell F scale
Rockwell 30T scale
Shear Strength
(ksi)
Section Size
(in)
Cold Work
(%)
Rod1/2 HardH0243   Typ
40   Typ
20   Typ
43   Typ
50   Typ
26   Typ
0.520
H0242   Typ
39   Typ
35   Typ
42   Typ
25   Typ
215
H0243   Typ
40   Typ
18   Typ
43   Typ
26   Typ
0.2520
H0242   Typ
40   Typ
25   Typ
42   Typ
25   Typ
120
1/8 HardH0038   Typ
30   Typ
26   Typ
36   Typ
44   Typ
25   Typ
0.56
HardH0448   Typ
44   Typ
20   Typ
48   Typ
27   Typ
135
H0453   Typ
49   Typ
10   Typ
54   Typ
29   Typ
0.2545
H0448   Typ
44   Typ
15   Typ
48   Typ
27   Typ
0.535
Nominal Grain Size 0.015 mmOS01533   Typ
11   Typ
46   Typ
43   Typ
22   Typ
0.5
Nominal Grain Size 0.050 mmOS05032   Typ
10   Typ
50   Typ
40   Typ
22   Typ
1
TubeLight Drawn, Light Cold RolledH5540   Typ
32   Typ
20   Typ
35   Typ
24   Typ
0.06515
Nominal Grain Size 0.050 mmOS05032   Typ
10   Typ
40   Typ
40   Typ
22   Typ
0.065
Wire1/2 HardH0251   Typ
41   Typ
6   Typ
27   Typ
0.08
1/8 HardH0038   Typ
30   Typ
20   Typ
25   Typ
0.08
HardH0456   Typ
51   Typ
3   Typ
30   Typ
0.08
Nominal Grain Size 0.035 mmOS03533   Typ
11   Typ
40   Typ
22   Typ
0.08
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1967
Melting Point - Solidus°F1924
Densitylb/cu in. at 68°F0.323
Specific Gravity8.94
Electrical Conductivity% IACS at 68°F85
Coefficient of Thermal Expansion 68-21210⁻⁶ per °F (68 – 212°F)9.5
Coefficient of Thermal Expansion 68-39210⁻⁶ per °F (68 – 392°F)9.7
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)9.9
Specific Heat CapacityBtu/ lb /°F at 68°F0.092
Modulus of Elasticity in Tensionksi17000
Modulus of Rigidityksi6400
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingGood
Oxyacetylene WeldingFair
Gas Shielded Arc WeldingFair
Coated Metal Arc WeldingNot Recommended
Spot WeldNot Recommended
Seam WeldNot Recommended
Butt WeldFair
Capacity for Being Cold WorkedGood
Capacity for Being Hot FormedGood
Forgeability Rating65
Machinability Rating85
Common Fabrication Processes
  • Cold - Drawing, machining, moderate cold heading
  • Hot - Extrusion, forging (closed die only)
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing8001200
Hot Treatment14001600
Typical uses
Product Category Product Reason Category Reason
ArchitectureFire ProtectionCorrosion ResistanceCorrosion Resistance
Fire ProtectionMachining CharacteristicsMachinability
ElectricalElectrical ConnectorsConductivity (Electrical)Electrical Conductivity
Electrical ConnectorsConductivity (Thermal)Thermal Conductivity
Electrical ConnectorsCorrosion ResistanceCorrosion Resistance
Electrical ConnectorsMachining CharacteristicsMachinability
Motor PartsCorrosion ResistanceCorrosion Resistance
Motor PartsMachining CharacteristicsMachinability
Soldering CopperCorrosion ResistanceCorrosion Resistance
Soldering CopperSoftening ResistanceResistance to Thermal Softening
Switch PartsConductivity (Electrical)Electrical Conductivity
Switch PartsConductivity (Thermal)Thermal Conductivity
Switch PartsCorrosion ResistanceCorrosion Resistance
Switch PartsMachining CharacteristicsMachinability
Transistor BasesConductivity (Electrical)Electrical Conductivity
Transistor BasesConductivity (Thermal)Thermal Conductivity
Transistor BasesCorrosion ResistanceCorrosion Resistance
Transistor BasesMachining CharacteristicsMachinability
IndustrialForgingsCorrosion ResistanceCorrosion Resistance
ForgingsMachining CharacteristicsMachinability
ForgingsSoftening ResistanceResistance to Thermal Softening
Furnace Brazed ArticlesCorrosion ResistanceCorrosion Resistance
Furnace Brazed ArticlesMachining CharacteristicsMachinability
Furnace Brazed ArticlesSoftening ResistanceResistance to Thermal Softening
Screw Machine ProductsCorrosion ResistanceCorrosion Resistance
Screw Machine ProductsMachining CharacteristicsMachinability
Welding Torch TipsConductivity (Electrical)Electrical Conductivity
Welding Torch TipsMachining CharacteristicsMachinability
Welding Torch TipsSoftening ResistanceResistance to Softening
PlumbingPlumbing FittingsCorrosion ResistanceCorrosion Resistance
Plumbing FittingsForming CharacteristicsFormability
Plumbing FittingsMachining CharacteristicsMachinability
Plumbing FittingsSolderabilitySolderability
Sprinkler HeadsCorrosion ResistanceCorrosion Resistance
Sprinkler HeadsMachining CharacteristicsMachinability
Applicable Specifications
Form System Standard Description
ASTMB224Standard Classification of Coppers
BarASTMB301/B301MFREE-CUTTING COPPER ROD AND BAR
Refinery ShapesASTMB5HIGH CONDUCTIVITY TOUGH-PITCH COPPER REFINERY SHAPES
RodASTMB301/B301MFREE-CUTTING COPPER ROD AND BAR
ShapesASTMB216REFINERY SHAPES, TOUGH-PITCH FIRE-REFINED
ASTMB301/B301MFREE-CUTTING COPPER ROD AND BAR
WireASTMB301/B301MFREE-CUTTING COPPER ROD AND BAR
Corrosion Properties

No information available.