Find suppliers for this alloy
C14530
| Elements | ||||
|---|---|---|---|---|
| Cu(1) | Sn | P | Te(2) | |
|
(1) Includes Ag + Sn + Te + Se (2) Tellurium and/or Selenium |
||||
| Min (%) | 99.90 | 0.003 | 0.001 | 0.003 |
| Max (%) | 0.023 | 0.010 | 0.023 | |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Section Size (in) |
|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||
| Flat Products | 1/2 Hard | H02 |
45 Typ |
39 Typ |
12 Typ |
0.02 |
| 1/2 Hard | H02 |
45 Typ |
39 Typ |
2.5 Typ |
0.003 | |
| 1/4 Hard | H01 |
40 Typ |
28 Typ |
5 Typ |
0.003 | |
| 1/4 Hard | H01 |
40 Typ |
28 Typ |
23 Typ |
0.02 | |
| 3/4 Hard | H03 |
48 Typ |
45 Typ |
6 Typ |
0.02 | |
| 3/4 Hard | H03 |
48 Min |
45 Min |
2 Typ |
0.003 | |
| Extra Hard | H06 |
55 Typ |
53 Typ |
1 Typ |
0.003 | |
| Extra Hard | H06 |
55 Typ |
53 Typ |
2 Typ |
0.02 | |
| Extra Spring | H10 |
59 Min |
58 Min |
1 Typ |
0.02 | |
| Extra Spring | H10 |
59 Min |
58 Min |
0.5 Typ |
0.003 | |
| Hard | H04 |
51 Typ |
49 Typ |
3 Typ |
0.02 | |
| Hard | H04 |
51 Typ |
49 Typ |
1.5 Typ |
0.003 | |
| Nominal Grain Size 0.015 mm | OS015 |
33 Typ |
12 Typ |
15 Typ |
0.003 | |
| Nominal Grain Size 0.015 mm | OS015 |
33 Typ |
12 Typ |
40 Typ |
0.02 | |
| Spring | H08 |
59 Typ |
58 Typ |
0.5 Typ |
0.003 | |
| Spring | H08 |
59 Typ |
58 Typ |
1 Typ |
0.02 | |
| Melting Point - Liquidus°F | 1976 |
|---|---|
| Melting Point - Solidus°F | 1926 |
| Densitylb/cu in. at 68°F | 0.323 |
| Specific Gravity | 8.94 |
| Electrical Conductivity% IACS at 68°F | 96 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 225 |
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 9.4 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 9.6 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.8 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.092 |
| Modulus of Elasticity in Tensionksi | 17000 |
| Modulus of Rigidityksi | 6400 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Good |
| Gas Shielded Arc Welding | Excellent |
| Coated Metal Arc Welding | Not Recommended |
| Spot Weld | Not Recommended |
| Seam Weld | Not Recommended |
| Butt Weld | Good |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Excellent |
| Forgeability Rating | 65 |
| Machinability Rating | 20 |
Common Fabrication Processes
- Blanking
- Bonding
- Deep Drawing
- Etching
- Forming
- Piercing
- Punching
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 840 | 1110 | ||
| Hot Working Temperature | 1400 | 1600 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Automotive | Electrical Connectors - Automotive | Conductivity (Electrical) | Electrical Conductivity |
| Electrical Connectors - Automotive | Conductivity (Thermal) | Thermal Conductivity | |
| Electrical Connectors - Automotive | Corrosion Resistance | Corrosion Resistance | |
| Electrical Connectors - Automotive | Finishing Characteristics | Ease of Tin Coating | |
| Electrical Connectors - Automotive | Forming Characteristics | Cold Workability | |
| Electrical Connectors - Automotive | Forming Characteristics | Formability | |
| Electrical Connectors - Automotive | Mechanical Properties | Strength vs. Copper | |
| Fins, Auto Radiator | Conductivity (Electrical) | Electrical Conductivity | |
| Fins, Auto Radiator | Conductivity (Thermal) | High Thermal Conductivity | |
| Fins, Auto Radiator | Conductivity (Thermal) | Thermal Conductivity | |
| Fins, Auto Radiator | Corrosion Resistance | Corrosion Resistance | |
| Fins, Auto Radiator | Corrosion Resistance | Corrosion Resistance to Hydrogen Embrittlement | |
| Fins, Auto Radiator | Forming Characteristics | Excellent Bending Capabilities | |
| Fins, Auto Radiator | Forming Characteristics | Excellent Formability | |
| Fins, Auto Radiator | Softening Resistance | Anneal Resistance | |
| Fins, Heat Exchanger | Conductivity (Electrical) | Electrical Conductivity | |
| Fins, Heat Exchanger | Conductivity (Thermal) | High Thermal Conductivity | |
| Fins, Heat Exchanger | Conductivity (Thermal) | Thermal Conductivity | |
| Fins, Heat Exchanger | Corrosion Resistance | Corrosion Resistance | |
| Fins, Heat Exchanger | Corrosion Resistance | Corrosion Resistance to Hydrogen Embrittlement | |
| Fins, Heat Exchanger | Forming Characteristics | Excellent Bending Capabilities | |
| Fins, Heat Exchanger | Forming Characteristics | Excellent Formability | |
| Fins, Heat Exchanger | Softening Resistance | Anneal Resistance | |
| Junction Boxes - Automotive | Conductivity (Electrical) | Electrical Conductivity | |
| Junction Boxes - Automotive | Conductivity (Thermal) | Thermal Conductivity | |
| Junction Boxes - Automotive | Corrosion Resistance | Corrosion Resistance | |
| Junction Boxes - Automotive | Forming Characteristics | Cold Workability | |
| Junction Boxes - Automotive | Mechanical Properties | Strength vs. Copper | |
| Electrical | Electrical Connectors - Modular Construction | Conductivity (Electrical) | Electrical Conductivity |
| Electrical Connectors - Modular Construction | Conductivity (Thermal) | Thermal Conductivity | |
| Electrical Connectors - Modular Construction | Corrosion Resistance | Corrosion Resistance | |
| Electrical Connectors - Modular Construction | Finishing Characteristics | Ease of Tin Coating | |
| Electrical Connectors - Modular Construction | Forming Characteristics | Cold Workability | |
| Electrical Connectors - Modular Construction | Forming Characteristics | Formability | |
| Electrical Connectors - Modular Construction | Mechanical Properties | Strength vs. Copper |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Sheet, Strip, Roller Bar & Plate | ASME | SB152 | COPPER SHEET, STRIP, PLATE, AND ROLLED BAR | ||
| Strip | ASTM | B888/B88M | COPPER ALLOY STRIP FOR USE IN MANUFACTURE OF ELECTRICAL CONNECTORS OR SPRING CONTACTS | ||
| ASTM | B152/B152M | COPPER SHEET, STRIP, PLATE AND ROLLED BAR |
Corrosion Properties