Find suppliers for this alloy
C14710
| Elements | ||||
|---|---|---|---|---|
| Cu(1,2) | Pb(3) | P(4) | S(5) | |
|
(1) Includes oxygen-free or deoxidized grades with deoxidizers (such as phosphorus boron lithium or others in an amount agreed upon. (2) Includes Ag, S, P, and Pb (3) Includes Ag, S, P, and Pb (4) Includes Ag, S, P, and Pb (5) Includes Ag, S, P, and Pb |
||||
| Min (%) | 99.90 | 0.010 | 0.05 | |
| Max (%) | 0.05 | 0.030 | 0.15 | |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Rockwell F scale | Rockwell 30T scale | Shear Strength (ksi) |
Section Size (in) |
Cold Work (%) |
|---|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||||||||
| Rod | 1/2 Hard | H02 |
43 Typ |
40 Typ |
20 Typ |
43 Typ |
50 Typ |
26 Typ |
0.5 | 20 | |
| 1/8 Hard | H00 |
38 Typ |
30 Typ |
26 Typ |
36 Typ |
44 Typ |
25 Typ |
0.5 | 6 | ||
| Extra Hard | H06 |
57 Typ |
55 Typ |
8 Typ |
29 Typ |
0.375 | 56 | ||||
| Hard | H04 |
48 Typ |
44 Typ |
12 Typ |
48 Typ |
27 Typ |
0.5 | 35 | |||
| Hard | H04 |
48 Typ |
44 Typ |
10 Typ |
45 Typ |
27 Typ |
0.25 | 36 | |||
| Hard | H04 |
40 Typ |
36 Typ |
15 Typ |
25 Typ |
1.75 | 24 | ||||
| Hard | H04 |
42 Typ |
38 Typ |
20 Typ |
26 Typ |
1.625 | 25 | ||||
| Hard | H04 |
46 Typ |
43 Typ |
11 Typ |
46 Typ |
27 Typ |
1 | 29 | |||
| Nominal Grain Size 0.015 mm | OS015 |
33 Typ |
11 Typ |
50 Typ |
43 Typ |
22 Typ |
0.5 | ||||
| Nominal Grain Size 0.050 mm | OS050 |
32 Typ |
10 Typ |
52 Typ |
40 Typ |
22 Typ |
0.5 | ||||
| (1)Volume and weight basis. | |
| Melting Point - Liquidus°F | 1969 |
|---|---|
| Melting Point - Solidus°F | 1953 |
| Densitylb/cu in. at 68°F | 0.323 |
| Specific Gravity | 8.94 |
| Electrical Conductivity% IACS at 68°F | 95 (1) |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 216 |
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 9.4 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 9.6 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.8 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.092 |
| Modulus of Elasticity in Tensionksi | 17000 |
| Modulus of Rigidityksi | 6400 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Not Recommended |
| Coated Metal Arc Welding | Not Recommended |
| Spot Weld | Not Recommended |
| Seam Weld | Not Recommended |
| Butt Weld | Good |
| Capacity for Being Cold Worked | Good |
| Capacity for Being Hot Formed | Excellent |
| Forgeability Rating | 65 |
| Machinability Rating | 85 |
Common Fabrication Processes
- Cold working
- Drawing
- Extruding
- Forging
- Hot working
- Machining
- Rolling
- Swaging
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 800 | 1200 | ||
| Hot Working Temperature | 1400 | 1400 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Electrical | Electrical Connectors | Conductivity (Electrical) | Electrical Conductivity |
| Electrical Connectors | Conductivity (Thermal) | Thermal Conductivity | |
| Electrical Connectors | Corrosion Resistance | Corrosion Resistance | |
| Electrical Connectors | Machining Characteristics | Machinability | |
| Electrical Connectors | Solderability | Solderability | |
| Motor Components | Conductivity (Electrical) | Electrical Conductivity | |
| Motor Components | Conductivity (Thermal) | Thermal Conductivity | |
| Motor Components | Corrosion Resistance | Corrosion Resistance | |
| Motor Components | Machining Characteristics | Machinability | |
| Motor Components | Solderability | Solderability | |
| Switch Components | Conductivity (Electrical) | Electrical Conductivity | |
| Switch Components | Conductivity (Thermal) | Thermal Conductivity | |
| Switch Components | Corrosion Resistance | Corrosion Resistance | |
| Switch Components | Machining Characteristics | Machinability | |
| Switch Components | Solderability | Solderability | |
| Fasteners | Rivets | Appearance | Color |
| Rivets | Corrosion Resistance | Corrosion Resistance | |
| Rivets | Machining Characteristics | Machinability | |
| Screws | Appearance | Color | |
| Screws | Corrosion Resistance | Corrosion Resistance | |
| Screws | Machining Characteristics | Machinability | |
| Industrial | Cold Forgings | Forming Characteristics | Formability |
| Cold Forgings | Machining Characteristics | Machinability | |
| Cold Headed Parts | Conductivity (Electrical) | Electrical Conductivity | |
| Cold Headed Parts | Conductivity (Thermal) | Thermal Conductivity | |
| Cold Headed Parts | Forming Characteristics | Formability | |
| Cold Headed Parts | Machining Characteristics | Machinability | |
| Furnace Brazed Articles | Brazing Characteristics | Brazability | |
| Furnace Brazed Articles | Conductivity (Thermal) | Thermal Conductivity | |
| Furnace Brazed Articles | Machining Characteristics | Machinability | |
| Furnace Brazed Articles | Softening Resistance | Resistance to Thermal Softening | |
| Screw Machine Products | Conductivity (Electrical) | Electrical Conductivity | |
| Screw Machine Products | Conductivity (Thermal) | Thermal Conductivity | |
| Screw Machine Products | Corrosion Resistance | Corrosion Resistance | |
| Screw Machine Products | Machining Characteristics | Machinability | |
| Soldering Coppers | Corrosion Resistance | Corrosion Resistance | |
| Soldering Coppers | Machining Characteristics | Machinability | |
| Soldering Coppers | Solderability | Solderability | |
| Welding Torch Tips | Conductivity (Thermal) | Thermal Conductivity | |
| Welding Torch Tips | Corrosion Resistance | Corrosion Resistance | |
| Welding Torch Tips | Machining Characteristics | Machinability | |
| Plumbing | Plumbing Fittings | Corrosion Resistance | Corrosion Resistance |
| Plumbing Fittings | Forming Characteristics | Formability | |
| Plumbing Fittings | Machining Characteristics | Machinability | |
| Plumbing Fittings | Solderability | Solderability |
Applicable Specifications