Find suppliers for this alloy
C15100
| Elements | ||
|---|---|---|
| Cu(1,2) | Zr | |
|
(1) Cu + Sum of Named Elements 99.9% min. (2) Cu value includes Ag. |
||
| Min (%) | 99.80 | 0.05 |
| Max (%) | 0.15 | |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Rockwell B scale | Rockwell F scale | Rockwell 30T scale | Section Size (in) |
|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||||||
| Flat Products | 1/2 Hard | H02 |
47 Typ |
45 Typ |
9 Typ |
37 Typ |
87 Typ |
56 Typ |
0.04 |
| 1/4 Hard | H01 |
42 Typ |
37 Typ |
13 Typ |
30 Typ |
81 Typ |
48 Typ |
0.04 | |
| 3/4 Hard | H03 |
51 Typ |
49 Typ |
6 Typ |
47 Typ |
90 Typ |
59 Typ |
0.04 | |
| Extra Hard | H06 |
63 Typ |
61 Typ |
3 Typ |
62 Typ |
64 Typ |
0.04 | ||
| Hard | H04 |
57 Typ |
55 Typ |
4 Typ |
57 Typ |
59 Typ |
61 Typ |
0.04 | |
| Nominal Grain Size 0.015 mm | OS015 |
38 Typ |
10 Typ |
36 Typ |
47 Typ |
0.04 | |||
| Spring | H08 |
68 Typ |
66 Typ |
2 Typ |
64 Typ |
65 Typ |
0.04 | ||
| Melting Point - Liquidus°F | 2008 |
|---|---|
| Melting Point - Solidus°F | 1886 |
| Densitylb/cu in. at 68°F | 0.323 |
| Specific Gravity | 8.94 |
| Electrical Conductivity% IACS at 68°F | 95 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 208 |
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 9.8 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 9.8 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.8 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.092 |
| Modulus of Elasticity in Tensionksi | 17500 |
| Modulus of Rigidityksi | 6730 |
| Poisson's Ratio | 0.3 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Good |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Not Recommended |
| Coated Metal Arc Welding | Not Recommended |
| Spot Weld | Not Recommended |
| Seam Weld | Not Recommended |
| Butt Weld | Good |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Excellent |
| Machinability Rating | 20 |
Common Fabrication Processes
- Blanking
- Cupping
- Deep Drawing
- Forming
- Piercing
- Stamping
Thermal Properties
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Electrical | Basses for Power Transmitters | Conductivity (Electrical) | Electrical Conductivity |
| Basses for Power Transmitters | Conductivity (Thermal) | Thermal Conductivity | |
| Basses for Power Transmitters | Corrosion Resistance | Corrosion Resistance | |
| Basses for Power Transmitters | Mechanical Properties | Retains Strength at High Temperatures | |
| Circuit Breakers, High Temperature | Conductivity (Electrical) | Electrical Conductivity | |
| Circuit Breakers, High Temperature | Conductivity (Thermal) | Thermal Conductivity | |
| Circuit Breakers, High Temperature | Corrosion Resistance | Corrosion Resistance | |
| Circuit Breakers, High Temperature | Mechanical Properties | Retains Strength at High Temperatures | |
| Commutators for Power Transmitters | Conductivity (Electrical) | Electrical Conductivity | |
| Commutators for Power Transmitters | Conductivity (Thermal) | Thermal Conductivity | |
| Commutators for Power Transmitters | Corrosion Resistance | Corrosion Resistance | |
| Commutators for Power Transmitters | Mechanical Properties | Retains Strength at High Temperatures | |
| Electrical Connectors | Conductivity (Electrical) | Electrical Conductivity | |
| Electrical Connectors | Conductivity (Thermal) | Thermal Conductivity | |
| Electrical Connectors | Corrosion Resistance | Corrosion Resistance | |
| Electrical Connectors | Softening Resistance | Resistance to Thermal Softening | |
| Electrical Connectors | Thermal Properties | Resistance to Stress Relaxation | |
| Electronic Circuits | Conductivity (Electrical) | Electrical Conductivity | |
| Electronic Circuits | Conductivity (Thermal) | Thermal Conductivity | |
| Electronic Circuits | Corrosion Resistance | Corrosion Resistance | |
| Electronic Circuits | Mechanical Properties | Retains Strength at High Temperatures | |
| Lead Frames | Conductivity (Electrical) | Electrical Conductivity | |
| Lead Frames | Conductivity (Thermal) | Thermal Conductivity | |
| Lead Frames | Corrosion Resistance | Corrosion Resistance | |
| Lead Frames | Softening Resistance | Resistance to Thermal Softening | |
| Lead Frames | Thermal Properties | Resistance to Stress Relaxation | |
| Rectifiers | Conductivity (Electrical) | Electrical Conductivity | |
| Rectifiers | Conductivity (Thermal) | Thermal Conductivity | |
| Rectifiers | Corrosion Resistance | Corrosion Resistance | |
| Rectifiers | Mechanical Properties | Retains Strength at High Temperatures | |
| Soldering and Welding Tips | Conductivity (Electrical) | Electrical Conductivity | |
| Soldering and Welding Tips | Conductivity (Thermal) | Thermal Conductivity | |
| Soldering and Welding Tips | Corrosion Resistance | Corrosion Resistance | |
| Soldering and Welding Tips | Mechanical Properties | Retains Strength at High Temperatures | |
| Switch Blade Jaws | Conductivity (Electrical) | Electrical Conductivity | |
| Switch Blade Jaws | Conductivity (Thermal) | Thermal Conductivity | |
| Switch Blade Jaws | Corrosion Resistance | Corrosion Resistance | |
| Switch Blade Jaws | Mechanical Properties | Moderate Strength | |
| Switch Blade Jaws | Mechanical Properties | Retains Strength at High Temperatures | |
| Switches | Conductivity (Electrical) | Electrical Conductivity | |
| Switches | Conductivity (Thermal) | Thermal Conductivity | |
| Switches | Corrosion Resistance | Corrosion Resistance | |
| Switches | Mechanical Properties | Retains Strength at High Temperatures |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Sheet | ASTM | B747 | COPPER-ZIRCONIUM ALLOY SHEET AND STRIP | ||
| Strip | ASTM | B888/B88M | COPPER ALLOY STRIP FOR USE IN MANUFACTURE OF ELECTRICAL CONNECTORS OR SPRING CONTACTS | ||
| ASTM | B747 | COPPER-ZIRCONIUM ALLOY SHEET AND STRIP |
Corrosion Properties