Find suppliers for this alloy
C15630
| Elements | |||
|---|---|---|---|
| Cu(1) | P | Ni | |
|
(1) Cu + Sum of Named Elements 99.5% min. |
|||
| Min (%) | 0.015 | 0.60 | |
| Max (%) | Rem | 0.040 | 0.90 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||
| Tube | Annealed | O61 |
29.7 Min |
8 Min |
40 Min |
| Melting Point - Liquidus°F | 2156 |
|---|---|
| Melting Point - Solidus°F | 1985 |
| Densitylb/cu in. at 68°F | 0.323 |
| Specific Gravity | 8.94 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.8 |
| Modulus of Elasticity in Tensionksi | 17000 |
| Modulus of Rigidityksi | 6400 |
| Magnetic Permeability | 0.8 |
| Poisson's Ratio | 0.35 |
| Technique | Suitability |
|---|---|
| Soldering | Good |
| Brazing | Good |
| Oxyacetylene Welding | Good |
| Gas Shielded Arc Welding | Good |
| Coated Metal Arc Welding | Good |
| Spot Weld | Poor |
| Seam Weld | Poor |
| Butt Weld | Poor |
| Capacity for Being Cold Worked | Good |
| Capacity for Being Hot Formed | Good |
| Machinability Rating | 20 |