Find suppliers for this alloy
C15650
| Elements | |||
|---|---|---|---|
| Cu(1) | P | Co | |
|
(1) Cu value includes Ag. |
|||
| Min (%) | 99.9 | 0.015 | 0.04 |
| Max (%) | 0.040 | 0.06 | |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||
| Tube | Anneal | ANNEAL |
41.5 Typ |
45 Min |
|
| Hard | H04 |
66 Typ |
6 Min |
||
| Melting Point - Solidus°F | 1974 |
|---|---|
| Densitylb/cu in. at 68°F | 0.321 |
| Specific Gravity | 8.94 |
| Electrical Conductivity% IACS at 68°F | 85 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 210 |
Fabrication Properties
Common Fabrication Processes
Thermal Properties
Typical Uses
Applicable Specifications
Corrosion Properties