Find suppliers for this alloyC16200
Chemical Composition
Element
Cu(1,2)FeCd
(1) Cu + Sum of Named Elements 99.5% min. (2) Cu value includes Ag.
Min (%)0.7
Max (%)Rem0.021.2
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.2% Offset
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell F scale
Shear Strength
(ksi)
Fatigue Strength**
(ksi)
Section Size
(in)
Cold Work
(%)
Flat ProductsExtra SpringH1072   Typ
59   Typ
1   Typ
75   Typ
0.04
HardH0460   Typ
45   Typ
5   Typ
64   Typ
0.04
Nominal Grain Size 0.025 mmOS02535   Typ
11   Typ
52   Typ
54   Typ
0.04
SpringH0864   Typ
3   Typ
73   Typ
0.04
Flat Products & WireSpringH0880   Typ
66   Typ
2   Typ
0.08
Flat Products, Rod & BarHardH0473   Typ
69   Typ
9   Typ
0.5
H0460   Typ
45   Typ
5   Typ
0.04
H0470   Typ
55   Typ
6   Typ
0.08
Rod1/2 HardH0258   Typ
45   Typ
12   Typ
65   Typ
0.525
HardH0473   Typ
70   Typ
69   Typ
9   Typ
73   Typ
56   Typ
30   Typ
0.5
Nominal Grain Size 0.050 mmOS05035   Typ
6.8   Typ
7   Typ
56   Typ
46   Typ
27   Typ
15   Typ
0.5
WireHardH0470   Typ
55   Typ
6   Typ
0.08
Hard DrawnH80100   Typ
1   Typ
0.0199
H8088   Typ
1.5   Typ
0.0896
Nominal Grain Size 0.025 mmOS02538   Typ
12   Typ
50   Typ
0.08
SpringH0880   Typ
66   Typ
2   Typ
0.08
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
Melting Point - Liquidus°F1969
Melting Point - Solidus°F1886
Densitylb/cu in. at 68°F0.321
Specific Gravity8.89
Electrical Conductivity% IACS at 68°F90
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F208
Coefficient of Thermal Expansion 68-21210⁻⁶ per °F (68 – 212°F)9.4
Coefficient of Thermal Expansion 68-39210⁻⁶ per °F (68 – 392°F)9.6
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)9.8
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi17000
Modulus of Rigidityksi6400
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingGood
Gas Shielded Arc WeldingGood
Coated Metal Arc WeldingNot Recommended
Spot WeldNot Recommended
Seam WeldNot Recommended
Butt WeldGood
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedGood
Machinability Rating20
Common Fabrication Processes
  • Drawing
  • Etching
  • Forming and Bending
  • Heading and Upsetting
  • Hot forging
  • Piercing
  • Punching
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing8001400
Hot Treatment14001600
Typical uses
Product Category Product Reason Category Reason
ConsumerElectric Blanket ElementsConductivity (Electrical)Electrical Conductivity
Electric Blanket ElementsConductivity (Thermal)Thermal Conductivity
Electric Blanket ElementsMechanical PropertiesHigh Strength
Electric Blanket ElementsMechanical PropertiesSpring Properties
ElectricalCable WrapConductivity (Electrical)Electrical Conductivity
Cable WrapConductivity (Thermal)Thermal Conductivity
Cable WrapCorrosion ResistanceCorrosion Resistance
Cable WrapMechanical PropertiesModerate Strength
Cable WrapSolderabilitySolderability
ClampsConductivity (Electrical)Electrical Conductivity
ClampsConductivity (Thermal)Thermal Conductivity
ClampsCorrosion ResistanceCorrosion Resistance
ClampsMechanical PropertiesModerate Strength
ConnectorsConductivity (Electrical)Electrical Conductivity
ConnectorsConductivity (Thermal)Thermal Conductivity
ConnectorsCorrosion ResistanceCorrosion Resistance
ConnectorsMechanical PropertiesModerate Strength
ConnectorsSolderabilitySolderability
ConnectorsWelding CharacteristicsArc Erosion Resistant
ContactsConductivity (Electrical)Electrical Conductivity
ContactsConductivity (Thermal)Thermal Conductivity
ContactsCorrosion ResistanceCorrosion Resistance
ContactsMechanical PropertiesModerate Strength
ContactsSolderabilitySolderability
Current Carrying RingsConductivity (Electrical)Electrical Conductivity
Current Carrying RingsConductivity (Thermal)Thermal Conductivity
Current Carrying RingsCorrosion ResistanceCorrosion Resistance
Current Carrying RingsMechanical PropertiesModerate Strength
Current Carrying RingsWelding CharacteristicsArc Erosion Resistant
FittingsCorrosion ResistanceCorrosion Resistance
FittingsMechanical PropertiesModerate Strength
Fuse ClipsConductivity (Electrical)Electrical Conductivity
Fuse ClipsConductivity (Thermal)Thermal Conductivity
Fuse ClipsCorrosion ResistanceCorrosion Resistance
Fuse ClipsMechanical PropertiesHigh Strength
Fuse ClipsSoftening ResistanceResistance to Thermal Softening
Fuse ClipsThermal PropertiesResistance to Stress Relaxation
Heating Pad ElementsConductivity (Electrical)Electrical Conductivity
Heating Pad ElementsConductivity (Thermal)Thermal Conductivity
Heating Pad ElementsForming CharacteristicsFormability
Heating Pad ElementsMechanical PropertiesModerate Strength
High Strength Transmission LinesConductivity (Electrical)Electrical Conductivity
High Strength Transmission LinesConductivity (Thermal)Thermal Conductivity
High Strength Transmission LinesCorrosion ResistanceCorrosion Resistance
High Strength Transmission LinesMechanical PropertiesHigh Strength
Rail bandsConductivity (Electrical)Electrical Conductivity
Rail bandsConductivity (Thermal)Thermal Conductivity
Rail bandsCorrosion ResistanceCorrosion Resistance
Rail bandsMechanical PropertiesModerate Strength
Rail bandsWelding CharacteristicsArc Erosion Resistant
Resistance and Spot Welding ElectrodesConductivity (Electrical)Electrical Conductivity
Resistance and Spot Welding ElectrodesConductivity (Thermal)Thermal Conductivity
Resistance and Spot Welding ElectrodesCorrosion ResistanceOxidation Resistance
Resistance and Spot Welding ElectrodesSoftening ResistanceResistance to Thermal Softening
Spring ContactsConductivity (Electrical)Electrical Conductivity
Spring ContactsConductivity (Thermal)Thermal Conductivity
Spring ContactsCorrosion ResistanceCorrosion Resistance
Spring ContactsMechanical PropertiesHigh Modulus of Elasticity
Spring ContactsMechanical PropertiesModerate Strength
Spring ContactsSolderabilitySolderability
Spring ContactsWelding CharacteristicsArc Erosion Resistant
Switch GearConductivity (Electrical)Electrical Conductivity
Switch GearConductivity (Thermal)Thermal Conductivity
Switch GearCorrosion ResistanceCorrosion Resistance
Switch GearMechanical PropertiesModerate Strength
Switch GearSoftening ResistanceResistance to Thermal Softening
Switch GearThermal PropertiesResistance to Stress Relaxation
Tinsel for the Telephone IndustryConductivity (Electrical)Electrical Conductivity
Tinsel for the Telephone IndustryConductivity (Thermal)Thermal Conductivity
Tinsel for the Telephone IndustryCorrosion ResistanceCorrosion Resistance
Tinsel for the Telephone IndustryMechanical PropertiesModerate Strength
Trolley WireConductivity (Electrical)Electrical Conductivity
Trolley WireConductivity (Thermal)Thermal Conductivity
Trolley WireCorrosion ResistanceCorrosion Resistance
Trolley WireMechanical PropertiesModerate Strength
Trolley WireMechanical PropertiesSpring Properties
Wave Guide CavitiesConductivity (Electrical)Electrical Conductivity
Wave Guide CavitiesConductivity (Thermal)Thermal Conductivity
Wave Guide CavitiesCorrosion ResistanceCorrosion Resistance
Wave Guide CavitiesSolderabilitySolderability
Wire for Telephone Cord SetsConductivity (Electrical)Electrical Conductivity
Wire for Telephone Cord SetsConductivity (Thermal)Thermal Conductivity
Wire for Telephone Cord SetsCorrosion ResistanceCorrosion Resistance
Wire for Telephone Cord SetsMechanical PropertiesModerate Strength
Wire for Telephone Cord SetsMechanical PropertiesSpring Properties
IndustrialBack Up BarsConductivity (Electrical)Electrical Conductivity
Back Up BarsConductivity (Thermal)Thermal Conductivity
Back Up BarsCorrosion ResistanceCorrosion Resistance
Back Up BarsMechanical PropertiesModerate Strength
Back Up BarsMechanical PropertiesRetains Strength at High Temperatures
Back Up BarsWelding CharacteristicsArc Erosion Resistant
Resistance Welding TipsConductivity (Electrical)Electrical Conductivity
Resistance Welding TipsConductivity (Thermal)Thermal Conductivity
Resistance Welding TipsSoftening ResistanceResistance to Softening
Resistance Welding TipsWelding CharacteristicsResistance to Deformation During Resistance Welding
Structural Parts in Resistance Welding MachinesConductivity (Electrical)Electrical Conductivity
Structural Parts in Resistance Welding MachinesConductivity (Thermal)Thermal Conductivity
Structural Parts in Resistance Welding MachinesCorrosion ResistanceCorrosion Resistance
Structural Parts in Resistance Welding MachinesMechanical PropertiesModerate Strength
Applicable Specifications
Form Sub-Form System Standard Description
Bar
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
Forgings
ForgingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
ForgingsSAEJ463WROUGHT COPPER AND COPPER ALLOYS
Rod
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
WireASTMB105HARD-DRAWN COPPER ALLOY WIRES FOR ELECTRICAL CONDUCTORS
ASTMB624HIGH-STRENGTH, HIGH-CONDUCTIVITY COPPER ALLOY WIRE FOR ELECTRONIC APPLICATIONS
MILITARYMIL-W-82598WIRE, COPPER-CADMIUM ALLOY
Corrosion Properties