Find suppliers for this alloyC17000
Chemical Composition
Element
Cu(1,2)AlBeCo(3)Si
(1) Cu value includes Ag. (2) Cu + Sum of Named Elements 99.5% min. (3) Ni + Co 0.20% min.: Ni + Fe + Co 0.6% max.
Min (%)1.600.20
Max (%)Rem0.201.850.20
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.2% Offset
Elongation
(%)
Rockwell B scale
Rockwell C scale
Rockwell 30T scale
Fatigue Strength**
(ksi)
Section Size
(in)
Flat Products1/2 Hard and Precipitation Heat TreatedTH02182   Typ
160   Typ
4   Typ
39   Typ
42   Typ
0.188
1/4 Hard and Precipitation Heat TreatedTH01172   Typ
150   Typ
5   Typ
37   Typ
40   Typ
0.188
Hard and Precipitation Heat TreatedTH04190   Typ
170   Typ
3   Typ
40   Typ
43   Typ
0.188
Mill-hardened Temper, TM - 1/2 HardTM00105   Typ
80   Typ
20   Typ
20   Typ
0.188
TM02128   Typ
105   Typ
15   Typ
27   Typ
0.188
TM01115   Typ
90   Typ
18   Typ
23   Typ
0.188
Mill-hardened Temper, TM - HardTM04142   Typ
122   Typ
12   Typ
32   Typ
0.188
Mill-hardened Temper, TM -XHM - Extra HardTM06168   Typ
148   Typ
6   Typ
36   Typ
0.188
Precipitation HardenedTF00165   Typ
145   Typ
7   Typ
35   Typ
36   Typ
0.188
Solution Heat TreatedTB0070   Typ
32   Typ
45   Typ
60   Typ
58   Typ
0.188
Solution Heat Treated and Cold Worked: 1/2 HardTD0292   Typ
82   Typ
15   Typ
92   Typ
77   Typ
0.188
Solution Heat Treated and Cold Worked: 1/4 HardTD0180   Typ
70   Typ
25   Typ
80   Typ
70   Typ
0.188
Solution Heat Treated and Cold Worked: HardTD04110   Typ
104   Typ
5   Typ
99   Typ
81   Typ
0.188
RodHard and Precipitation Heat TreatedTH04178   Typ
36   Typ
<1
TH04183   Typ
37   Typ
1
TH04188   Typ
38   Typ
0.375
Solution Heat Treated and Cold Worked: HardTD04105   Typ
95   Typ
1
TD04112   Typ
95   Typ
0.375
TD04100   Typ
95   Typ
<1
ShapesSolution Heat TreatedTB0085  
30  
60  
Solution Heat Treated and Cold Worked: HardTD04120  
110  
8  
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
(1) In the precipitation hardened condition.
Melting Point - Liquidus°F1800
Melting Point - Solidus°F1590
Densitylb/cu in. at 68°F0.304
Specific Gravity8.41
Electrical Conductivity% IACS at 68°F22(1)
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F62
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)9.9
Specific Heat CapacityBtu/ lb /°F at 68°F0.1
Modulus of Elasticity in Tensionksi18500
Modulus of Rigidityksi7300
Fabrication Properties
Technique Suitability
SolderingGood
BrazingGood
Oxyacetylene WeldingNot Recommended
Gas Shielded Arc WeldingGood
Coated Metal Arc WeldingGood
Spot WeldGood
Seam WeldFair
Butt WeldFair
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedGood
Machinability Rating20
Common Fabrication Processes
  • Blanking
  • Drawing
  • Drilling
  • Forming and Bending
  • Tapping
  • Turning
    
Thermal Properties
Treatment Minimum* Maximum* Value* Time** Medium
* Temperature is measured in Fahrenheit. ** Time is measured in minutes.
Stress Relief390
Solution Treatment142514750.5Water
Precipitation Treatment6003Air
Hot Treatment12001500
Typical uses
Product Category Product Reason Category Reason
ElectricalConnectorsConductivity (Electrical)Electrical Conductivity
ConnectorsConductivity (Thermal)Thermal Conductivity
ConnectorsCorrosion ResistanceCorrosion Resistance
ConnectorsMechanical PropertiesHigh Strength
ConnectorsSolderabilitySolderability
ConnectorsThermal PropertiesResistance to Stress Relaxation
Electronic Equipment ComponentsConductivity (Electrical)Electrical Conductivity
Electronic Equipment ComponentsConductivity (Thermal)Thermal Conductivity
Electronic Equipment ComponentsCorrosion ResistanceCorrosion Resistance
Electronic Equipment ComponentsMechanical PropertiesHigh Strength
Electronic Equipment ComponentsThermal PropertiesResistance to Stress Relaxation
Fuse ClipsConductivity (Electrical)Electrical Conductivity
Fuse ClipsConductivity (Thermal)Thermal Conductivity
Fuse ClipsCorrosion ResistanceCorrosion Resistance
Fuse ClipsMechanical PropertiesHigh Strength
Relay PartsConductivity (Electrical)Electrical Conductivity
Relay PartsConductivity (Thermal)Thermal Conductivity
Relay PartsCorrosion ResistanceCorrosion Resistance
Relay PartsMechanical PropertiesHigh Strength
Switch PartsConductivity (Electrical)Electrical Conductivity
Switch PartsConductivity (Thermal)Thermal Conductivity
Switch PartsCorrosion ResistanceCorrosion Resistance
Switch PartsMechanical PropertiesHigh Strength
Switch PartsThermal PropertiesResistance to Stress Relaxation
FastenersFastenersCorrosion ResistanceCorrosion Resistance
FastenersMechanical PropertiesHigh Strength
FastenersThermal PropertiesResistance to Stress Relaxation
Lock WashersCorrosion ResistanceCorrosion Resistance
Lock WashersMechanical PropertiesHigh Strength
Lock WashersThermal PropertiesResistance to Stress Relaxation
Retaining RingsCorrosion ResistanceCorrosion Resistance
Retaining RingsMechanical PropertiesHigh Strength
Retaining RingsThermal PropertiesResistance to Stress Relaxation
Roll PinsCorrosion ResistanceCorrosion Resistance
Roll PinsMechanical PropertiesHigh Strength
IndustrialBellowsForming CharacteristicsFormability
BellowsMechanical PropertiesDuctility
BellowsMechanical PropertiesHigh Strength
BellowsThermal PropertiesResistance to Stress Relaxation
Bourdon TubingForming CharacteristicsFormability
Bourdon TubingMechanical PropertiesDuctility
Bourdon TubingMechanical PropertiesHigh Strength
Bourdon TubingThermal PropertiesResistance to Stress Relaxation
DiaphragmsForming CharacteristicsFormability
DiaphragmsMechanical PropertiesDuctility
DiaphragmsMechanical PropertiesHigh Strength
DiaphragmsThermal PropertiesResistance to Stress Relaxation
Electrodes for WeldingConductivity (Electrical)Electrical Conductivity
Electrodes for WeldingConductivity (Thermal)Thermal Conductivity
Electrodes for WeldingMechanical PropertiesHigh Strength
ForgingsCorrosion ResistanceCorrosion Resistance
ForgingsForming CharacteristicsFormability
ForgingsMechanical PropertiesHigh Strength
Machined ComponentsCorrosion ResistanceCorrosion Resistance
Machined ComponentsMechanical PropertiesHigh Strength
Machined ComponentsThermal PropertiesResistance to Stress Relaxation
Plastic Mold ComponentsConductivity (Thermal)Thermal Conductivity
Plastic Mold ComponentsFriction & Wear PropertiesWear Resistance
Plastic Mold ComponentsMechanical PropertiesHigh Strength
Pump PartsCorrosion ResistanceCorrosion Resistance
Pump PartsFriction & Wear PropertiesWear Resistance
Pump PartsMechanical PropertiesHigh Strength
Rolling Mill PartsCorrosion ResistanceCorrosion Resistance
Rolling Mill PartsFriction & Wear PropertiesWear Resistance
Rolling Mill PartsMechanical PropertiesHigh Strength
Rolling Mill PartsMechanical PropertiesRetains Strength at High Temperatures
Rolling Mill PartsThermal PropertiesResistance to Stress Relaxation
Spline ShaftsCorrosion ResistanceCorrosion Resistance
Spline ShaftsMechanical PropertiesHigh Strength
SpringsCorrosion ResistanceCorrosion Resistance
SpringsMechanical PropertiesHigh Strength
SpringsThermal PropertiesResistance to Stress Relaxation
Steel Mold ComponentsConductivity (Thermal)Thermal Conductivity
Steel Mold ComponentsMechanical PropertiesHigh Strength
ValvesCorrosion ResistanceCorrosion Resistance
ValvesFriction & Wear PropertiesWear Resistance
ValvesMechanical PropertiesHigh Strength
Welding EquipmentConductivity (Electrical)Electrical Conductivity
Welding EquipmentConductivity (Thermal)Thermal Conductivity
Welding EquipmentCorrosion ResistanceCorrosion Resistance
Welding EquipmentCreep PropertiesCreep Resistant
Welding EquipmentFriction & Wear PropertiesWear Resistance
Welding EquipmentMechanical PropertiesVery High Strength
Welding EquipmentSoftening ResistanceResistance to Thermal Softening
OtherContinuous Casting, Permanent BrassConductivity (Thermal)Thermal Conductivity
Continuous Casting, Permanent BrassCorrosion ResistanceCorrosion Resistance
Continuous Casting, Permanent BrassMechanical PropertiesHigh Strength
Non-Sparking ToolsDamping CharacteristicsEnergy Damping
Non-Sparking ToolsImpact ResistanceImpact Resistant
Non-Sparking ToolsMagnetic PropertiesNon-Magnetic
Non-Sparking ToolsMechanical PropertiesHigh Strength
Non-Sparking ToolsNon-SparkingNon-Sparking
Applicable Specifications
Form Sub-Form Specific Sub-Form System Standard Description
BarASTMB194COPPER BERYLLIUM ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
ASTMB196/B196MCOPPER BERYLLIUM ALLOY ROD AND BAR
ExtrusionsExtrusionsASTMB570COPPER-BERYLLIUM ALLOY FORGINGS AND EXTRUSIONS
ForgingsForgingsASTMB570COPPER-BERYLLIUM ALLOY FORGINGS AND EXTRUSIONS
PlateASTMB194COPPER BERYLLIUM ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
RodASTMB196/B196MCOPPER BERYLLIUM ALLOY ROD AND BAR
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
SheetASTMB194COPPER BERYLLIUM ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
StripASTMB194COPPER BERYLLIUM ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
Electric Connector & Spring ContactASTMB888/B88MCOPPER ALLOY STRIP FOR USE IN MANUFACTURE OF ELECTRICAL CONNECTORS OR SPRING CONTACTS
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
Corrosion Properties

No information available.