Chemical Composition
Element
Cu(1,2)AlBeCo(3)Si
(1) Cu + Sum of Named Elements 99.5% min. (2) Cu value includes Ag. (3) Ni + Co 0.20% min.: Ni + Fe + Co 0.6% max.
Min (%)1.800.20
Max (%)Rem0.202.000.20
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.2% Offset
Elongation
(%)
Rockwell B scale
Rockwell C scale
Rockwell 30T scale
Torsion Modulus
(ksi)
Fatigue Strength**
(ksi)
Section Size
(in)
Flat Products1/2 Hard and Precipitation Heat TreatedTH02195   Typ
175   Typ
3   Typ
41   Typ
44   Typ
0.188
1/4 Hard and Precipitation Heat TreatedTH01185   Typ
165   Typ
4   Typ
40   Typ
40   Typ
0.188
Hard and Precipitation Heat TreatedTH04200   Typ
180   Typ
2   Typ
42   Typ
45   Typ
0.188
Mill-hardened Temper, TM - 1/2 HardTM02128   Typ
105   Typ
15   Typ
27   Typ
0.188
TM00105   Typ
82   Typ
20   Typ
27   Typ
0.188
TM01115   Typ
92   Typ
17   Typ
23   Typ
0.188
Mill-hardened Temper, TM - HardTM04142   Typ
122   Typ
12   Typ
32   Typ
0.188
Mill-hardened Temper, TM - SHMTM05150   Min
125   Min
9   Min
31   Min
Mill-hardened Temper, TM - XHMS SpringTM08182   Typ
160   Typ
6   Typ
0.188
Mill-hardened Temper, TM -XHM - Extra HardTM06168   Typ
148   Typ
7   Typ
37   Typ
0.188
Precipitation HardenedTF00175   Typ
155   Typ
6   Typ
38   Typ
36   Typ
0.188
Solution Heat TreatedTB0070   Typ
32   Typ
45   Typ
60   Typ
58   Typ
Solution Heat Treated and Cold Worked: 1/2 HardTD0292   Typ
82   Typ
15   Typ
92   Typ
77   Typ
0.188
Solution Heat Treated and Cold Worked: 1/4 HardTD0180   Typ
70   Typ
25   Typ
80   Typ
70   Typ
0.188
Solution Heat Treated and Cold Worked: HardTD04110   Typ
104   Typ
5   Typ
99   Typ
81   Typ
0.188
RodHard and Precipitation Heat TreatedTH04205   Typ
160   Typ
2   Typ
42   Typ
0.375
TH04200   Typ
155   Typ
2   Typ
41   Typ
0.375
TH04195   Typ
145   Typ
4   Typ
41   Typ
7.3   Typ
3
Precipitation HardenedTF00182   Typ
130   Typ
3   Typ
39   Typ
55   Typ
3
TF00182   Typ
145   Typ
4   Typ
39   Typ
Solution Heat TreatedTB0072   Typ
20   Typ
20   Typ
65   Typ
Solution Heat Treated and Cold Worked: HardTD04110   Typ
75   Typ
8   Typ
95   Typ
0.375
TD04103   Typ
75   Typ
8   Typ
94   Typ
3
TD04108   Typ
75   Typ
8   Typ
95   Typ
1
Wire1/2 Hard and Precipitation Heat TreatedTH02200   Typ
185   Typ
1   Typ
1/4 Hard and Precipitation Heat TreatedTH01190   Typ
175   Typ
2   Typ
3/4 Hard and Precipitation Heat TreatedTH03210   Typ
195   Typ
1   Typ
Hard and Precipitation Heat TreatedTH04212   Typ
195   Typ
1   Typ
Precipitation HardenedTF00178   Typ
160   Typ
3   Typ
Solution Heat TreatedTB0068   Typ
28   Typ
35   Typ
Solution Heat Treated and Cold Worked: 1/2 HardTD02122   Typ
100   Typ
5   Typ
Solution Heat Treated and Cold Worked: 1/4 HardTD01102   Typ
82   Typ
10   Typ
Solution Heat Treated and Cold Worked: 3/4 HardTD03142   Typ
120   Typ
2   Typ
Solution Heat Treated and Cold Worked: HardTD04152   Typ
125   Typ
1   Typ
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
(1) In the precipitation hardened condition.
(2) Actual value is 62-75.
Melting Point - Liquidus°F1800
Melting Point - Solidus°F1590
Densitylb/cu in. at 68°F0.29
Specific Gravity8.26
Electrical Conductivity% IACS at 68°F22(1)
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F62(2)
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)9.9
Specific Heat CapacityBtu/ lb /°F at 68°F0.1
Modulus of Elasticity in Tensionksi18500
Modulus of Rigidityksi7300
Fabrication Properties
Technique Suitability
SolderingGood
BrazingGood
Oxyacetylene WeldingNot Recommended
Gas Shielded Arc WeldingGood
Coated Metal Arc WeldingGood
Spot WeldGood
Seam WeldFair
Butt WeldFair
Capacity for Being Cold WorkedGood
Capacity for Being Hot FormedExcellent
Forgeability Rating40
Machinability Rating20
Common Fabrication Processes
  • Blanking
  • Drawing
  • Drilling
  • Forming and Bending
  • Tapping
  • Turning
    
Thermal Properties
Treatment Minimum* Maximum* Value* Time** Medium
* Temperature is measured in Fahrenheit. ** Time is measured in minutes.
Stress Relief400
Solution Treatment142514750.5Water
Precipitation Treatment6003Air
Hot Treatment12001500
Typical uses
Product Category Product Reason Category Reason
ElectricalBelleville WashersCorrosion ResistanceCorrosion Resistance
Belleville WashersForming CharacteristicsFormability, Good
Belleville WashersMechanical PropertiesHigh Strength
Belleville WashersMechanical PropertiesLow Elastic Modulus
ClipsConductivity (Electrical)Electrical Conductivity
ClipsConductivity (Thermal)Thermal Conductivity
ClipsCorrosion ResistanceCorrosion Resistance
ClipsMechanical PropertiesVery High Strength
ConnectorsConductivity (Electrical)Electrical Conductivity
ConnectorsConductivity (Thermal)Thermal Conductivity
ConnectorsCreep PropertiesCreep Resistant
ConnectorsMechanical PropertiesVery High Strength
ConnectorsSoftening ResistanceResistance to Thermal Softening
ConnectorsThermal PropertiesResistance to Stress Relaxation
Contact BridgesConductivity (Electrical)Electrical Conductivity
Contact BridgesConductivity (Thermal)Thermal Conductivity
Contact BridgesCorrosion ResistanceCorrosion Resistance
Contact BridgesMechanical PropertiesVery High Strength
Electrical Switch and Relay BladesConductivity (Electrical)Electrical Conductivity
Electrical Switch and Relay BladesForming CharacteristicsFormability, Good
Electrical Switch and Relay BladesHeat TreatabilityHeat Treatable
Electrical Switch and Relay BladesMechanical PropertiesFatigue Life
Electrical Switch and Relay BladesMechanical PropertiesHigh Endurance Limit
Electrical Switch and Relay BladesMechanical PropertiesHigh Strength
Electrical Switch and Relay BladesThermal PropertiesResistance to Stress Relaxation
Fuse ClipsConductivity (Electrical)Electrical Conductivity
Fuse ClipsConductivity (Thermal)Thermal Conductivity
Fuse ClipsCorrosion ResistanceCorrosion Resistance
Fuse ClipsMechanical PropertiesVery High Strength
Navigational InstrumentsConductivity (Electrical)Electrical Conductivity
Navigational InstrumentsConductivity (Thermal)Thermal Conductivity
Navigational InstrumentsCorrosion ResistanceCorrosion Resistance
Navigational InstrumentsMechanical PropertiesVery High Strength
Relay PartsConductivity (Electrical)Electrical Conductivity
Relay PartsConductivity (Thermal)Thermal Conductivity
Relay PartsCorrosion ResistanceCorrosion Resistance
Relay PartsMechanical PropertiesVery High Strength
Spring Connectors, Current CarryingConductivity (Electrical)Electrical Conductivity
Spring Connectors, Current CarryingConductivity (Thermal)Thermal Conductivity
Spring Connectors, Current CarryingCorrosion ResistanceCorrosion Resistance
Spring Connectors, Current CarryingCreep PropertiesCreep Resistant
Spring Connectors, Current CarryingMechanical PropertiesVery High Strength
Spring Connectors, Current CarryingSoftening ResistanceResistance to Thermal Softening
Spring Connectors, Current CarryingThermal PropertiesResistance to Stress Relaxation
Switch PartsConductivity (Electrical)Electrical Conductivity
Switch PartsConductivity (Thermal)Thermal Conductivity
Switch PartsCorrosion ResistanceCorrosion Resistance
Switch PartsCreep PropertiesCreep Resistant
Switch PartsMechanical PropertiesVery High Strength
Switch PartsSoftening ResistanceResistance to Thermal Softening
FastenersBoltsCorrosion ResistanceCorrosion Resistance
BoltsCreep PropertiesCreep Resistant
BoltsMechanical PropertiesVery High Strength
BoltsSoftening ResistanceResistance to Thermal Softening
FastenersCorrosion ResistanceCorrosion Resistance
FastenersMechanical PropertiesToughness
FastenersMechanical PropertiesVery High Strength
Lock WashersCorrosion ResistanceCorrosion Resistance
Lock WashersMechanical PropertiesDuctility
Lock WashersMechanical PropertiesVery High Strength
Retaining RingsCorrosion ResistanceCorrosion Resistance
Retaining RingsForming CharacteristicsFormability
Retaining RingsMechanical PropertiesVery High Strength
Roll PinsCorrosion ResistanceCorrosion Resistance
Roll PinsMechanical PropertiesFatigue Resistance
Roll PinsMechanical PropertiesVery High Strength
ScrewsCorrosion ResistanceCorrosion Resistance
ScrewsCreep PropertiesCreep Resistant
ScrewsMechanical PropertiesVery High Strength
ScrewsSoftening ResistanceResistance to Thermal Softening
WashersCorrosion ResistanceCorrosion Resistance
WashersMechanical PropertiesVery High Strength
IndustrialBearingsCorrosion ResistanceCorrosion Resistance
BearingsFriction & Wear PropertiesGalling Resistance
BearingsFriction & Wear PropertiesWear Resistance
BearingsMachining CharacteristicsMachinability
BearingsMechanical PropertiesHigh Strength
BellowsCorrosion ResistanceCorrosion Resistance
BellowsForming CharacteristicsFormability, Good
BellowsMechanical PropertiesHigh Strength
BellowsMechanical PropertiesLow Elastic Modulus
Bourdon TubesCorrosion ResistanceCorrosion Resistance
Bourdon TubesForming CharacteristicsFormability, Good
Bourdon TubesMechanical PropertiesHigh Strength
Bourdon TubesMechanical PropertiesLow Elastic Modulus
BushingsCorrosion ResistanceCorrosion Resistance
BushingsFriction & Wear PropertiesGalling Resistance
BushingsFriction & Wear PropertiesWear Resistance
BushingsMachining CharacteristicsMachinability
BushingsMechanical PropertiesHigh Strength
DiaphragmsCorrosion ResistanceCorrosion Resistance
DiaphragmsForming CharacteristicsFormability, Good
DiaphragmsMechanical PropertiesHigh Strength
DiaphragmsMechanical PropertiesLow Elastic Modulus
Flexible Metal HoseForming CharacteristicsFormability
Flexible Metal HoseMechanical PropertiesDuctility
Flexible Metal HoseMechanical PropertiesVery High Strength
Housings for InstrumentsCorrosion ResistanceCorrosion Resistance
Housings for InstrumentsMachining CharacteristicsMachinability
Housings for InstrumentsMagnetic PropertiesNon-Magnetic
Housings for InstrumentsMechanical PropertiesHigh Strength
Non Sparking Safety ToolsMechanical PropertiesVery High Strength
Non Sparking Safety ToolsNon-SparkingNon-Sparking
Pump PartsCorrosion ResistanceCorrosion Resistance
Pump PartsForming CharacteristicsFormability
Pump PartsMechanical PropertiesFatigue Resistance
Pump PartsMechanical PropertiesVery High Strength
PumpsCorrosion ResistanceCorrosion Resistance
PumpsMechanical PropertiesVery High Strength
Rolling Mill PartsCorrosion ResistanceCorrosion Resistance
Rolling Mill PartsForming CharacteristicsFormability
Rolling Mill PartsFriction & Wear PropertiesWear Resistance
Rolling Mill PartsMechanical PropertiesFatigue Resistance
Rolling Mill PartsMechanical PropertiesVery High Strength
ShaftsCorrosion ResistanceCorrosion Resistance
ShaftsMechanical PropertiesVery High Strength
Spline ShaftsCorrosion ResistanceCorrosion Resistance
Spline ShaftsForming CharacteristicsFormability
Spline ShaftsFriction & Wear PropertiesWear Resistance
Spline ShaftsMechanical PropertiesVery High Strength
SpringsCorrosion ResistanceCorrosion Resistance
SpringsForming CharacteristicsFormability
SpringsMechanical PropertiesFatigue Resistance
SpringsMechanical PropertiesVery High Strength
Springs, ElectrochemicalConductivity (Electrical)Electrical Conductivity
Springs, ElectrochemicalConductivity (Thermal)Thermal Conductivity
Springs, ElectrochemicalCorrosion ResistanceCorrosion Resistance
Springs, ElectrochemicalMechanical PropertiesHigh Modulus of Elasticity
Valve SeatsCorrosion ResistanceCorrosion Resistance
Valve SeatsForging CharacteristicsForgability
Valve SeatsFriction & Wear PropertiesGalling Resistance
Valve SeatsFriction & Wear PropertiesWear Resistance
Valve SeatsMechanical PropertiesDuctility
Valve SeatsMechanical PropertiesHigh Strength
Valve StemsCorrosion ResistanceCorrosion Resistance
Valve StemsForging CharacteristicsForgability
Valve StemsFriction & Wear PropertiesGalling Resistance
Valve StemsFriction & Wear PropertiesWear Resistance
Valve StemsMechanical PropertiesDuctility
Valve StemsMechanical PropertiesHigh Strength
ValvesCorrosion ResistanceCorrosion Resistance
ValvesForming CharacteristicsFormability
ValvesMechanical PropertiesVery High Strength
Wear Plates on Heavy EquipmentCorrosion ResistanceCorrosion Resistance
Wear Plates on Heavy EquipmentFriction & Wear PropertiesGalling Resistance
Wear Plates on Heavy EquipmentFriction & Wear PropertiesWear Resistance
Wear Plates on Heavy EquipmentMachining CharacteristicsMachinability
Wear Plates on Heavy EquipmentMechanical PropertiesHigh Strength
Welding EquipmentConductivity (Electrical)Electrical Conductivity
Welding EquipmentConductivity (Thermal)Thermal Conductivity
Welding EquipmentCorrosion ResistanceCorrosion Resistance
Welding EquipmentCreep PropertiesCreep Resistant
Welding EquipmentMechanical PropertiesVery High Strength
Welding EquipmentSoftening ResistanceResistance to Thermal Softening
OrdnanceFiring PinsCorrosion ResistanceCorrosion Resistance
Firing PinsMechanical PropertiesVery High Strength
OtherToolsDamping CharacteristicsEnergy Damping
ToolsImpact ResistanceImpact Resistant
ToolsMagnetic PropertiesNon-Magnetic
ToolsMechanical PropertiesHigh Strength
ToolsNon-SparkingNon-Sparking
Applicable Specifications
Form Sub-Form Specific Sub-Form Temper System Standard Description
BarPrecipitation HardenedAMS4533COPPER BERYLLINUM ALLOY BARS AND RODS, SOLUTION AND PRECIPITATION HEAT TREATED
Hard and Precipitation Heat TreatedAMS4534COPPER BERYLLIUM ALLOY BARS AND RODS, SOLUTION HEAT TREATED, COLD WORKED AND PRECIPITATION HEAT TREA
Solution Heat TreatedAMS4650COPPER-BERYLLIUM ALLOY BARS, RODS AND FORGINGS, SOLUTION HEAT TREATED
Solution Heat Treated and Cold Worked: HardAMS4651COPER-BERYLLIUM ALLOY BARS AND RODS, HARD TEMPER
ASTMB194COPPER BERYLLIUM ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
ASTMB196/B196MCOPPER BERYLLIUM ALLOY ROD AND BAR
MILITARYMIL-C-21657COPPER-BERYLLIUM ALLOY, LOW MAGNETIC EFFECT (FOR SPECIAL PURPOSE TOOLS AND EQUIPMENT)
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
ExtrusionsExtrusionsASTMB570COPPER-BERYLLIUM ALLOY FORGINGS AND EXTRUSIONS
ForgingsSolution Heat TreatedAMS4650COPPER-BERYLLIUM ALLOY BARS, RODS AND FORGINGS, SOLUTION HEAT TREATED
ForgingsASTMB570COPPER-BERYLLIUM ALLOY FORGINGS AND EXTRUSIONS
PlateSolution Heat TreatedAMS4530COPPER-BERYLLIUM ALLOY SHEET, STRIP, AND PLATE - SOLUTION TREATED
ASTMB194COPPER BERYLLIUM ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
RodPrecipitation HardenedAMS4533COPPER BERYLLINUM ALLOY BARS AND RODS, SOLUTION AND PRECIPITATION HEAT TREATED
Hard and Precipitation Heat TreatedAMS4534COPPER BERYLLIUM ALLOY BARS AND RODS, SOLUTION HEAT TREATED, COLD WORKED AND PRECIPITATION HEAT TREA
Solution Heat TreatedAMS4650COPPER-BERYLLIUM ALLOY BARS, RODS AND FORGINGS, SOLUTION HEAT TREATED
Solution Heat Treated and Cold Worked: HardAMS4651COPER-BERYLLIUM ALLOY BARS AND RODS, HARD TEMPER
ASTMB196/B196MCOPPER BERYLLIUM ALLOY ROD AND BAR
MILITARYMIL-C-21657COPPER-BERYLLIUM ALLOY, LOW MAGNETIC EFFECT (FOR SPECIAL PURPOSE TOOLS AND EQUIPMENT)
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
ShapesSolution Heat TreatedAMS4650COPPER-BERYLLIUM ALLOY BARS, RODS AND FORGINGS, SOLUTION HEAT TREATED
SheetSolution Heat TreatedAMS4530COPPER-BERYLLIUM ALLOY SHEET, STRIP, AND PLATE - SOLUTION TREATED
1/2 HardAMS4532COPPER BERYLLIUM ALOY SHEET AND STRIP, HALF-HARD
ASTMB194COPPER BERYLLIUM ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
StripSolution Heat TreatedAMS4530COPPER-BERYLLIUM ALLOY SHEET, STRIP, AND PLATE - SOLUTION TREATED
1/2 HardAMS4532COPPER BERYLLIUM ALOY SHEET AND STRIP, HALF-HARD
ASTMB194COPPER BERYLLIUM ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
Electric Connector & Spring ContactASTMB888/B88MCOPPER ALLOY STRIP FOR USE IN MANUFACTURE OF ELECTRICAL CONNECTORS OR SPRING CONTACTS
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
TubePrecipitation HardenedAMS4535COPPER BERYLLIUM ALLOY MECHANICAL TUBING, SOLUTION AND PRECIPITATION HEAT TREATED
SeamlessASTMB643COPPER-BERYLLIUM ALLOY SEAMLESS TUBE
WireAMS4725COPPER-BERYLLIUM ALLOY WIRE - SOLUTION HEAT TREATED
ASTMB197/B197MCOPPER BERYLLIUM ALLOY WIRE
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
Corrosion Properties

No information available.