Find suppliers for this alloyC17510
Chemical Composition
Element
Cu(1,2)FeNiAlBeCoSi
(1) Cu + Sum of Named Elements 99.5% min. (2) Cu value includes Ag.
Min (%)1.40.2
Max (%)Rem0.102.20.200.60.30.20
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.2% Offset
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell 30T scale
Fatigue Strength**
(ksi)
Section Size
(in)
Flat Products1/2 Hard and Precipitation Heat TreatedTH02115   Typ
108   Typ
8   Typ
98   Typ
81   Typ
35   Typ
Hard and Precipitation Heat TreatedTH04115   Typ
110   Typ
8   Typ
98   Typ
81   Typ
Precipitation HardenedTF00110   Typ
90   Typ
12   Typ
96   Typ
80   Typ
Solution Heat TreatedTB0045   Typ
25   Typ
28   Typ
32   Typ
36   Typ
Solution Heat Treated and Cold Worked: 1/2 HardTD0268   Typ
60   Typ
8   Typ
70   Typ
64   Typ
Solution Heat Treated and Cold Worked: HardTD0478   Typ
70   Typ
5   Typ
83   Typ
72   Typ
ForgingsPrecipitation HardenedTF00115   Typ
90   Typ
92   Typ
4
Solution Heat TreatedTB0042   Typ
20   Typ
50   Typ
RodHard and Precipitation Heat TreatedTH04115   Typ
110   Typ
14   Typ
98   Typ
Precipitation HardenedTF00110   Typ
90   Typ
18   Typ
96   Typ
Solution Heat TreatedTB0045   Typ
25   Typ
28   Typ
35   Typ
Solution Heat Treated and Cold Worked: HardTD0472   Typ
65   Typ
12   Typ
68   Typ
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
(1) Cold worked and precipitation hardened condition. HT Temper
(2) AT Temper
Melting Point - Liquidus°F1955
Melting Point - Solidus°F1885
Densitylb/cu in. at 68°F0.317
Specific Gravity8.77
Electrical Conductivity% IACS at 68°F48(1)
Electrical Conductivity% IACS at 68°F45(2)
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F120
Coefficient of Thermal Expansion 68-39210⁻⁶ per °F (68 – 392°F)9.8
Specific Heat CapacityBtu/ lb /°F at 68°F0.1
Modulus of Elasticity in Tensionksi19200
Modulus of Rigidityksi7500
Fabrication Properties
Technique Suitability
SolderingGood
BrazingGood
Oxyacetylene WeldingNot Recommended
Gas Shielded Arc WeldingFair
Coated Metal Arc WeldingFair
Spot WeldGood
Seam WeldFair
Butt WeldFair
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedGood
Common Fabrication Processes
  • Blanking
  • Drilling
  • Forming and Bending
  • Tapping
  • Turning
    
Thermal Properties
Treatment Minimum* Maximum* Value* Time** Medium
* Temperature is measured in Fahrenheit. ** Time is measured in minutes.
Solution Treatment155017001Water
Precipitation Treatment8503Air
Hot Treatment12001750
Typical uses
Product Category Product Reason Category Reason
ElectricalConductorsConductivity (Electrical)Electrical Conductivity
ConductorsCorrosion ResistanceCorrosion Resistance
ConductorsCreep PropertiesCreep Resistant
ConductorsMechanical PropertiesHigh Strength
ConductorsSoftening ResistanceResistance to Thermal Softening
ConductorsSolderabilitySolderability
Connectors, Heavy DutyConductivity (Electrical)Electrical Conductivity
Connectors, Heavy DutyConductivity (Thermal)Thermal Conductivity
Connectors, Heavy DutyCorrosion ResistanceCorrosion Resistance
Connectors, Heavy DutyCreep PropertiesCreep Resistant
Connectors, Heavy DutyMechanical PropertiesHigh Strength
Connectors, Heavy DutyMechanical PropertiesRetains Strength at High Temperatures
Connectors, Heavy DutySoftening ResistanceResistance to Thermal Softening
Fuse ClipsConductivity (Electrical)Electrical Conductivity
Fuse ClipsCorrosion ResistanceCorrosion Resistance
Fuse ClipsMechanical PropertiesHigh Strength
Fuse ClipsSolderabilitySolderability
Instrument PartsAppearanceAppearance
Instrument PartsConductivity (Electrical)Electrical Conductivity
Instrument PartsCorrosion ResistanceCorrosion Resistance
Instrument PartsMechanical PropertiesHigh Strength
Instrument PartsSolderabilitySolderability
Relay PartsConductivity (Electrical)Electrical Conductivity
Relay PartsCorrosion ResistanceCorrosion Resistance
Relay PartsCreep PropertiesCreep Resistant
Relay PartsMechanical PropertiesHigh Strength
Relay PartsSoftening ResistanceResistance to Thermal Softening
Relay PartsSolderabilitySolderability
Switch PartsConductivity (Electrical)Electrical Conductivity
Switch PartsCorrosion ResistanceCorrosion Resistance
Switch PartsCreep PropertiesCreep Resistant
Switch PartsMechanical PropertiesHigh Strength
Switch PartsSoftening ResistanceResistance to Thermal Softening
Switch PartsSolderabilitySolderability
FastenersFastenersCorrosion ResistanceCorrosion Resistance
FastenersMechanical PropertiesHigh Strength
IndustrialDie casting plunger tipsConductivity (Thermal)Thermal Conductivity
Die casting plunger tipsMechanical PropertiesHigh Strength
Die casting plunger tipsMechanical PropertiesRetains Strength at High Temperatures
High Flux ElectromagnetsConductivity (Electrical)Electrical Conductivity
High Flux ElectromagnetsConductivity (Thermal)Thermal Conductivity
High Flux ElectromagnetsCorrosion ResistanceCorrosion Resistance
High Flux ElectromagnetsMagnetic PropertiesNon-Magnetic
High Flux ElectromagnetsMechanical PropertiesHigh Strength
SpringsCorrosion ResistanceCorrosion Resistance
SpringsMechanical PropertiesFatigue Resistance
SpringsMechanical PropertiesHigh Modulus of Elasticity
SpringsMechanical PropertiesHigh Strength
Thermal Transfer PlatesConductivity (Thermal)Thermal Conductivity
Thermal Transfer PlatesCorrosion ResistanceCorrosion Resistance
Thermal Transfer PlatesMechanical PropertiesHigh Strength
Welding EquipmentConductivity (Electrical)Electrical Conductivity
Welding EquipmentConductivity (Thermal)Thermal Conductivity
Welding EquipmentCorrosion ResistanceCorrosion Resistance
Welding EquipmentCreep PropertiesCreep Resistant
Welding EquipmentMechanical PropertiesHigh Strength
Welding EquipmentSoftening ResistanceResistance to Thermal Softening
Applicable Specifications
Form Specific Sub-Form System Standard Description
BarASTMB441COPPER-COBALT-BERYLLIUM (UNS NO. C17500) AND COPPER-NICKEL-BERYLLIUM (UNS NO. C17510) ROD AND BAR
ASTMB534COPPER-COBALT-BERYLLIUM ALLOY, PLATE, SHEET, STRIP, AND ROLLED BAR
Extrusions
Forgings
Forgings & ExtrusionsASTMB870COPPER-BERYLLIUM ALLOY FORGINGS AND EXTRUSION ALLOYS (UNS Nos. C17500 AND C17510)
Heat Exchanger TubeASTMB944COPPER-BERYLLIUM WELDED HEAT EXCHANGER AND CONDENSER TUBE UNS No. C175100
PlateASTMB534COPPER-COBALT-BERYLLIUM ALLOY, PLATE, SHEET, STRIP, AND ROLLED BAR
RodASTMB441COPPER-COBALT-BERYLLIUM (UNS NO. C17500) AND COPPER-NICKEL-BERYLLIUM (UNS NO. C17510) ROD AND BAR
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
Seamless TubeASTMB937COPPER-BERYLLIUM SEAMLESS TUBE (UNS Nos.17500 and 17510)
ShapesSAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
SheetASTMB534COPPER-COBALT-BERYLLIUM ALLOY, PLATE, SHEET, STRIP, AND ROLLED BAR
StripASTMB534COPPER-COBALT-BERYLLIUM ALLOY, PLATE, SHEET, STRIP, AND ROLLED BAR
Electric Connector & Spring ContactASTMB888/B88MCOPPER ALLOY STRIP FOR USE IN MANUFACTURE OF ELECTRICAL CONNECTORS OR SPRING CONTACTS
MILITARYMIL-C-81021COPPER BERYLLIUM ALLOY (COPPER ALLOY NUMBERS C17500 AND C17510) STRIP
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
TubeSAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
Corrosion Properties

No information available.