Find suppliers for this alloy
C18085
| Elements | |||||
|---|---|---|---|---|---|
| Cu(1) | Ag | Cr | Si | Ti | |
|
(1) Cu + Sum of Named Elements 99.5% min. |
|||||
| Min (%) | 0.01 | 0.20 | 0.01 | 0.01 | |
| Max (%) | Rem | 0.30 | 1.0 | 0.50 | 0.8 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Vickers Hardness, 3000 gm |
|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||
| Strip | TH04 |
78 Min 80 Typ 83 Max |
72.5 Min 77 Typ 78 Max |
150 Typ |
|
| Melting Point - Liquidus°F | 1976 |
|---|---|
| Densitylb/cu in. at 68°F | 0.321 |
| Specific Gravity | 8.89 |
| Electrical Conductivity% IACS at 68°F | 80 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 330 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 10.0 |
| Modulus of Elasticity in Tensionksi | 21 |
| Poisson's Ratioksi | 0.3 |