Find suppliers for this alloy
C18400
| Elements | |||||||||
|---|---|---|---|---|---|---|---|---|---|
| Cu(1,2) | Zn | Fe | P | As | Ca | Cr | Li | Si | |
|
(1) Cu value includes Ag. (2) Cu + Sum of Named Elements 99.5% min. |
|||||||||
| Min (%) | 0.40 | ||||||||
| Max (%) | Rem | 0.7 | 0.15 | 0.05 | 0.005 | 0.005 | 1.2 | 0.05 | 0.10 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Rockwell F scale | Section Size (in) |
Cold Work (%) |
|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||||||
| Flat Products | 1/4 Hard and Precipitation Heat Treated | TH01 |
67 Typ |
59 Typ |
14 Typ |
79 Typ |
0.04 | 50 | |
| Precipitation Hardened | TF00 |
51 Typ |
36 Typ |
22 Typ |
59 Typ |
0.04 | |||
| Solution Heat Treated | TB00 |
34 Typ |
19 Typ |
40 Typ |
16 Typ |
0.04 | |||
| Solution Heat Treated and Cold Worked: 1/8 Hard | TD00 |
53 Typ |
51 Typ |
6 Typ |
66 Typ |
0.04 | 50 | ||
| Plate | Precipitation Hardened | TF00 |
56 Typ |
40 Typ |
30 Typ |
68 Typ |
3 | ||
| Precipitation Hardened | TF00 |
58 Typ |
42 Typ |
25 Typ |
70 Typ |
2 | |||
| Rod | 1/4 Hard and Precipitation Heat Treated | TH01 |
77 Typ |
67 Typ |
19 Typ |
83 Typ |
0.5 | 50 | |
| 1/4 Hard and Precipitation Heat Treated | TH01 |
77 Typ |
65 Typ |
16 Typ |
82 Typ |
0.5 | 60.5 | ||
| 1/4 Hard and Precipitation Heat Treated | TH01 |
74 Typ |
73 Typ |
5 Typ |
0.156 | 90 | |||
| Precipitation Hardened | TF00 |
70 Typ |
65 Typ |
18 Typ |
75 Typ |
2 | |||
| Precipitation Hardened | TF00 |
70 Typ |
55 Typ |
21 Typ |
70 Typ |
0.5 | |||
| Precipitation Hardened | TF00 |
72 Typ |
65 Typ |
18 Typ |
80 Typ |
1 | |||
| Precipitation Hardened | TF00 |
65 Typ |
55 Typ |
18 Typ |
70 Typ |
3 | |||
| Precipitation Hardened | TF00 |
55 Typ |
43 Typ |
25 Typ |
68 Typ |
4 | |||
| Solution Heat Treated | TB00 |
45 Typ |
14 Typ |
40 Typ |
0.5 | ||||
| Solution Heat Treated and Cold Worked: 1/8 Hard | TD00 |
57 Typ |
56 Typ |
11 Typ |
65 Typ |
0.5 | 60.5 | ||
| Solution Heat Treated and Cold Worked: 1/8 Hard | TD00 |
86 Typ |
77 Typ |
14 Typ |
0.156 | 91 | |||
| Tube | Annealed | O61 |
40 Typ |
15 Typ |
50 Typ |
59 Typ |
|||
| Solution Heat Treated and Cold Worked: 1/2 Hard | TD02 |
69 Typ |
63 Typ |
26 Typ |
84 Typ |
76 | |||
| Solution Heat Treated and Cold Worked: 1/8 Hard | TD00 |
59 Typ |
57 Typ |
21 Typ |
67 Typ |
76 | |||
| (1)Solution heat treated, cold worked (50% minimum) and aged.(2)Solution heat treated, cold worked (50% minimum) and aged. | |
| Melting Point - Liquidus°F | 1967 |
|---|---|
| Melting Point - Solidus°F | 1958 |
| Densitylb/cu in. at 68°F | 0.321 |
| Specific Gravity | 8.89 |
| Electrical Conductivity% IACS at 68°F | 80 (1) |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 187 (2) |
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 9.8 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.092 |
| Modulus of Elasticity in Tensionksi | 17000 |
| Modulus of Rigidityksi | 7200 |
| Technique | Suitability |
|---|---|
| Soldering | Good |
| Brazing | Good |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Good |
| Coated Metal Arc Welding | Not Recommended |
| Spot Weld | Not Recommended |
| Seam Weld | Not Recommended |
| Butt Weld | Fair |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Good |
| Forgeability Rating | 80 |
| Machinability Rating | 20 |
Common Fabrication Processes
- Bending
- Cold working
- Drawing
- Forging
- heading
- Hot working
- Impacting
- Rolling
- Swaging
| Treatment | Minimum* | Maximum* | Value* | Time** | Medium |
|---|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. ** Time is measured in minutes. | |||||
| Solution Treatment | 1800 | 1850 | 0.5 | Water | |
| Precipitation Treatment | 860 | 3 | Air | ||
| Hot Working Temperature | 1500 | 1700 | |||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Electrical | Arcing and Bridging Parts | Conductivity (Electrical) | Electrical Conductivity |
| Arcing and Bridging Parts | Conductivity (Thermal) | Thermal Conductivity | |
| Arcing and Bridging Parts | Corrosion Resistance | Corrosion Resistance | |
| Arcing and Bridging Parts | Welding Characteristics | Arc Erosion Resistant | |
| Cable Connectors | Conductivity (Electrical) | Electrical Conductivity | |
| Cable Connectors | Conductivity (Thermal) | Thermal Conductivity | |
| Cable Connectors | Corrosion Resistance | Corrosion Resistance | |
| Cable Connectors | Solderability | Solderability | |
| Circuit Breaker Parts | Conductivity (Electrical) | Electrical Conductivity | |
| Circuit Breaker Parts | Conductivity (Thermal) | Thermal Conductivity | |
| Circuit Breaker Parts | Corrosion Resistance | Corrosion Resistance | |
| Contacts | Conductivity (Electrical) | Electrical Conductivity | |
| Contacts | Conductivity (Thermal) | Thermal Conductivity | |
| Contacts | Forming Characteristics | Formability | |
| Contacts | Mechanical Properties | Moderate to High Strength | |
| Contacts | Mechanical Properties | Retains Strength at High Temperatures | |
| Current Carrying Arms and Shafts | Conductivity (Electrical) | Electrical Conductivity | |
| Current Carrying Arms and Shafts | Conductivity (Thermal) | Thermal Conductivity | |
| Current Carrying Arms and Shafts | Corrosion Resistance | Corrosion Resistance | |
| Current Carrying Arms and Shafts | Creep Properties | Creep Resistant | |
| Electric Motor Parts | Conductivity (Electrical) | Electrical Conductivity | |
| Electric Motor Parts | Conductivity (Thermal) | Thermal Conductivity | |
| Electric Motor Parts | Corrosion Resistance | Corrosion Resistance | |
| Electric Motor Parts | Forming Characteristics | Formability | |
| Electric Motor Parts | Mechanical Properties | Moderate to High Strength | |
| Electric Motor Parts | Mechanical Properties | Retains Strength at High Temperatures | |
| Electrical Conductors Requiring Greater Strength than Copper | Conductivity (Electrical) | Electrical Conductivity | |
| Electrical Conductors Requiring Greater Strength than Copper | Conductivity (Thermal) | Thermal Conductivity | |
| Electrical Conductors Requiring Greater Strength than Copper | Corrosion Resistance | Corrosion Resistance | |
| Electrical Conductors Requiring Greater Strength than Copper | Mechanical Properties | Moderate Strength | |
| Generator Components | Conductivity (Electrical) | Electrical Conductivity | |
| Generator Components | Conductivity (Thermal) | Thermal Conductivity | |
| Generator Components | Corrosion Resistance | Corrosion Resistance | |
| Generator Components | Forming Characteristics | Formability | |
| Generator Components | Mechanical Properties | Moderate to High Strength | |
| Generator Components | Mechanical Properties | Retains Strength at High Temperatures | |
| Grid Side rods in Electron Tubes | Conductivity (Electrical) | Electrical Conductivity | |
| Grid Side rods in Electron Tubes | Conductivity (Thermal) | Thermal Conductivity | |
| Grid Side rods in Electron Tubes | Corrosion Resistance | Corrosion Resistance | |
| Grid Side rods in Electron Tubes | Softening Resistance | Resistance to Thermal Softening | |
| Semi Conductor Bases | Conductivity (Electrical) | Electrical Conductivity | |
| Semi Conductor Bases | Conductivity (Thermal) | Thermal Conductivity | |
| Semi Conductor Bases | Corrosion Resistance | Corrosion Resistance | |
| Semi Conductor Bases | Forming Characteristics | Formability | |
| Semi Conductor Bases | Mechanical Properties | Moderate to High Strength | |
| Semi Conductor Bases | Mechanical Properties | Retains Strength at High Temperatures | |
| Switch Contacts | Conductivity (Electrical) | Electrical Conductivity | |
| Switch Contacts | Conductivity (Thermal) | Thermal Conductivity | |
| Switch Contacts | Corrosion Resistance | Corrosion Resistance | |
| Switch Contacts | Softening Resistance | Resistance to Thermal Softening | |
| Switch Contacts | Solderability | Solderability | |
| Switch Gears | Conductivity (Electrical) | Electrical Conductivity | |
| Switch Gears | Conductivity (Thermal) | Thermal Conductivity | |
| Switch Gears | Corrosion Resistance | Corrosion Resistance | |
| Switch Gears | Mechanical Properties | Moderate Strength | |
| Thermal Conductors Requiring Greater Strength than Copper | Conductivity (Electrical) | Electrical Conductivity | |
| Thermal Conductors Requiring Greater Strength than Copper | Conductivity (Thermal) | Thermal Conductivity | |
| Thermal Conductors Requiring Greater Strength than Copper | Corrosion Resistance | Corrosion Resistance | |
| Thermal Conductors Requiring Greater Strength than Copper | Mechanical Properties | Moderate Strength | |
| Wire, High Temperature | Conductivity (Electrical) | Electrical Conductivity | |
| Wire, High Temperature | Conductivity (Thermal) | Thermal Conductivity | |
| Wire, High Temperature | Corrosion Resistance | Corrosion Resistance | |
| Wire, High Temperature | Forming Characteristics | Formability | |
| Wire, High Temperature | Mechanical Properties | Moderate to High Strength | |
| Wire, High Temperature | Mechanical Properties | Retains Strength at High Temperatures | |
| Industrial | Electrode Holder Jaws | Conductivity (Electrical) | Electrical Conductivity |
| Electrode Holder Jaws | Conductivity (Thermal) | Thermal Conductivity | |
| Electrode Holder Jaws | Corrosion Resistance | Corrosion Resistance | |
| Electrode Holder Jaws | Creep Properties | Creep Resistant | |
| Electrode Holder Jaws | Softening Resistance | Resistance to Thermal Softening | |
| Flash Welding Electrodes | Conductivity (Electrical) | Electrical Conductivity | |
| Flash Welding Electrodes | Conductivity (Thermal) | Thermal Conductivity | |
| Flash Welding Electrodes | Corrosion Resistance | Oxidation Resistance | |
| Flash Welding Electrodes | Softening Resistance | Resistance to Thermal Softening | |
| Molds | Conductivity (Thermal) | Thermal Conductivity | |
| Molds | Corrosion Resistance | Corrosion Resistance | |
| Molds | Creep Properties | Creep Resistant | |
| Molds | Mechanical Properties | Moderate Strength | |
| Molds | Softening Resistance | Resistance to Thermal Softening | |
| Resistance Welding Electrodes | Conductivity (Electrical) | Electrical Conductivity | |
| Resistance Welding Electrodes | Conductivity (Thermal) | Thermal Conductivity | |
| Resistance Welding Electrodes | Corrosion Resistance | Oxidation Resistance | |
| Resistance Welding Electrodes | Softening Resistance | Resistance to Thermal Softening | |
| Resistance Welding Equipment | Conductivity (Electrical) | Electrical Conductivity | |
| Resistance Welding Equipment | Corrosion Resistance | Corrosion Resistance | |
| Resistance Welding Equipment | Mechanical Properties | Moderate Strength | |
| Seam Welding Wheels | Conductivity (Electrical) | Electrical Conductivity | |
| Seam Welding Wheels | Conductivity (Thermal) | Thermal Conductivity | |
| Seam Welding Wheels | Corrosion Resistance | Corrosion Resistance | |
| Seam Welding Wheels | Softening Resistance | Resistance to Thermal Softening | |
| Spot Welding Tips | Conductivity (Electrical) | Electrical Conductivity | |
| Spot Welding Tips | Conductivity (Thermal) | Thermal Conductivity | |
| Spot Welding Tips | Corrosion Resistance | Corrosion Resistance | |
| Spot Welding Tips | Creep Properties | Creep Resistant | |
| Spot Welding Tips | Softening Resistance | Resistance to Thermal Softening | |
| Other | Stressed Parts | Conductivity (Electrical) | Electrical Conductivity |
| Stressed Parts | Corrosion Resistance | Corrosion Resistance | |
| Stressed Parts | Mechanical Properties | Moderate Strength |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Bar | SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | ||
| MILITARY | MIL-C-19311 | COPPER-CHROMIUM-ALLOY FORGINGS, ROD, BAR, AND STRIP | |||
| SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |||
| Forgings | Forgings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |
| Forgings | SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | ||
| Forgings | MILITARY | MIL-C-19311 | COPPER-CHROMIUM-ALLOY FORGINGS, ROD, BAR, AND STRIP | ||
| Rod | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| MILITARY | MIL-C-19311 | COPPER-CHROMIUM-ALLOY FORGINGS, ROD, BAR, AND STRIP | |||
| SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | |||
| Strip | MILITARY | MIL-C-19311 | COPPER-CHROMIUM-ALLOY FORGINGS, ROD, BAR, AND STRIP |
Corrosion Properties