Find suppliers for this alloy
C18610
| Elements | |||||||
|---|---|---|---|---|---|---|---|
| Cu(1,2) | Fe | Ni | Co | Cr | Ti | Zr | |
|
(1) Cu value includes Ag. (2) Cu + Sum of Named Elements 99.5% min. |
|||||||
| Min (%) | 0.25 | 0.10 | 0.05 | 0.05 | |||
| Max (%) | Rem | 0.10 | 0.25 | 0.8 | 1.0 | 0.50 | 0.40 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||
| Flat Products | Mill-hardened Temper, TM - 1/2 Hard | TM02 |
76 Typ |
70 Typ |
11 Typ |
| Mill-hardened Temper, TM - Hard | TM04 |
84 Typ |
80 Typ |
8 Typ |
|
| Mill-hardened Temper, TM - XHMS Spring | TM08 |
94 Typ |
90 Typ |
6 Typ |
|
| Melting Point - Liquidus°F | 1995 |
|---|---|
| Melting Point - Solidus°F | 1960 |
| Densitylb/cu in. at 68°F | 0.321 |
| Specific Gravity | 8.89 |
| Electrical Conductivity% IACS at 68°F | 70 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 162 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.8 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 18500 |
| Modulus of Rigidityksi | 7000 |
| Magnetic Permeability | 0.9999 |
| Poisson's Ratio | 0.3 |
| Technique | Suitability |
|---|---|
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Excellent |
Common Fabrication Processes
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 660 | 1740 | ||
| Hot Working Temperature | 1400 | 1700 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Automotive | Connectors, automotive | Corrosion Resistance | Corrosion Resistance |
| Connectors, automotive | Mechanical Properties | Moderate Strength | |
| Consumer | Connector, appliance | Corrosion Resistance | Corrosion Resistance |
| Connector, appliance | Corrosion Resistance | Corrosion Resistance to Chemicals | |
| Connector, appliance | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Connector, appliance | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Connector, appliance | Forming Characteristics | Formability | |
| Connector, appliance | Mechanical Properties | Moderate Strength | |
| Industrial | Connector, chemical processing sensor | Corrosion Resistance | Corrosion Resistance |
| Connector, chemical processing sensor | Forming Characteristics | Formability | |
| Connector, chemical processing sensor | Friction & Wear Properties | Wear Resistance | |
| Connector, chemical processing sensor | Mechanical Properties | High Modulus of Elasticity | |
| Connector, chemical processing sensor | Mechanical Properties | Moderate Strength |
Applicable Specifications
Corrosion Properties