C18620
| Elements | ||||||
|---|---|---|---|---|---|---|
| Cu(1) | Sn | Zn | P | Ni | Co | |
|
(1) Cu value includes Ag. |
||||||
| Min (%) | 99.40 | 0.03 | 0.02 | 0.040 | 0.02 | 0.14 |
| Max (%) | 0.15 | 0.10 | 0.075 | 0.06 | 0.21 | |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Vickers Hardness, 500 gm |
|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||
| Pipe | Anneal | ANNEAL |
36 Min 43 Typ |
14 Min 21 Typ |
40 Typ |
85 Typ |
| Hard | H04 |
51 Min 72 Typ |
60 Min 69 Typ |
2 Typ |
85 Typ |
|
| Tube | Anneal | ANNEAL |
363 Min 43 Typ |
1421 Min 21 Typ |
40 Typ |
85 Typ |
| Hard | H04 |
51 Min 72 Typ |
60 Min 69 Typ |
2 Typ |
85 Typ |
|
| Melting Point - Liquidus°F | 1976 |
|---|---|
| Melting Point - Solidus°F | 1967 |
| Densitylb/cu in. at 68°F | 0.321 |
| Specific Gravity | 8.94 |
| Electrical Conductivity% IACS at 68°F | 85 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 196 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 10 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Spot Weld | Not Recommended |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Excellent |
| Forgeability Rating | 65 |
| Machinability Rating | 20 |
Common Fabrication Processes
Thermal Properties
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Automotive | Automotive & Aircraft-air,hydraulic, gas & oil lines | ||
| Consumer | Air Conditioner Tube, Steam Lines | ||
| Electrical | Heater Elements | ||
| Industrial | Evaproator Tube, Plumbing Tube |