Find suppliers for this alloy
C18625
| Elements | ||||||
|---|---|---|---|---|---|---|
| Cu(1,2) | Sn | Zn | P | Ni | Co | |
|
(1) Cu value includes Ag. (2) Cu + Sum of Named Elements 99.5% min. |
||||||
| Min (%) | 99.40 | .01 | .05 | .15 | ||
| Max (%) | .10 | .10 | .09 | .10 | .35 | |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Rockwell B scale | Section Size (in) |
|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||||
| Rod | Solution Heat Treated and Cold Worked: Hard | TD04 |
54 Min 61 Typ |
51 Min 58 Typ |
20 Min |
70 Typ |
.8 |
| Rod & Bar | Solution Heat Treated and Cold Worked: 1/2 Hard | TD02 |
44 Min 51 Typ |
39 Min 48 Typ |
25 Min |
60 Typ |
1 |
| Melting Point - Liquidus°F | 1976 |
|---|---|
| Melting Point - Solidus°F | 1967 |
| Densitylb/cu in. at 68°F | 0.32 |
| Specific Gravity | 8.9 |
| Electrical Conductivity% IACS at 68°F | 85 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 195 |
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 10 |
| Modulus of Elasticity in Tensionksi | 17400 |
| Modulus of Rigidityksi | 6500 |
| Poisson's Ratio | 0.33 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Excellent |
| Forgeability Rating | 80 |
| Machinability Rating | 20 |
Common Fabrication Processes
| Treatment | Minimum* | |||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 1110 | |||
| Hot Working Temperature | 930 | |||
| Stress Relief | 570 | |||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Automotive | Automotive electrical terminals | ||
| Connectors, automotive | |||
| Heater Cores | |||
| Relays | |||
| Sensor Bodies | |||
| Electrical | Connectors for High Temperatures | ||
| Electrical Conductors | |||
| Wire, Electrical |
Applicable Specifications
Corrosion Properties