Find suppliers for this alloyC19000
Chemical Composition
Element
Cu(1,2)PbZnFePNi
(1) Cu value includes Ag. (2) Cu + Sum of Named Elements 99.5% min.
Min (%)0.150.9
Max (%)Rem0.050.80.100.351.3
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.2% Offset
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Shear Strength
(ksi)
Section Size
(in)
Cold Work
(%)
Flat Products1/2 Hard and Stress RelievedHR0276   Typ
70   Typ
65   Typ
4   Typ
83   Typ
38   Typ
0.040
Extra Spring and Stress RelievedHR10100   Typ
91   Typ
77   Typ
2   Typ
94   Typ
50   Typ
0.040
Hard and Stress RelievedHR0484   Typ
77   Typ
72   Typ
3   Typ
88   Typ
42   Typ
0.040
Precipitation HardenedTF0065   Typ
40   Typ
40   Typ
25   Typ
72   Typ
35   Typ
0.040
RodHard and Stress RelievedHR0485   Typ
80   Typ
75   Typ
15   Typ
87   Typ
42   Typ
135
Precipitation HardenedTF0065   Typ
45   Typ
45   Typ
30   Typ
70   Typ
35   Typ
1
Solution Heat TreatedTB0038   Typ
20   Typ
20   Typ
50   Typ
45   Typ
25   Typ
1
Wire1/2 Hard and Stress RelievedHR0288   Typ
78   Typ
73   Typ
8   Typ
43   Typ
0.08
1/4 Hard and Stress RelievedHR0180   Typ
73   Typ
70   Typ
13   Typ
40   Typ
0.08
Extra Spring and Stress RelievedHR10115   Typ
101   Typ
81   Typ
3   Typ
60   Typ
0.08
Hard and Stress RelievedHR0497   Typ
85   Typ
77   Typ
5   Typ
49   Typ
0.08
Precipitation HardenedTF0065   Typ
40   Typ
40   Typ
25   Typ
35   Typ
0.08
Spring and Stress RelievedHR08110   Typ
97   Typ
80   Typ
4   Typ
57   Typ
0.08
* Measured at room temperature, 68°F (20°C).
Physical Properties
(1) Age hardened condition.
Melting Point - Liquidus°F1980
Melting Point - Solidus°F1900
Densitylb/cu in. at 68°F0.323
Specific Gravity8.94
Electrical Conductivity% IACS at 68°F60(1)
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F145
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)9.8
Specific Heat CapacityBtu/ lb /°F at 68°F0.092
Modulus of Elasticity in Tensionksi18000
Modulus of Rigidityksi6800
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingGood
Gas Shielded Arc WeldingGood
Coated Metal Arc WeldingNot Recommended
Spot WeldFair
Seam WeldFair
Butt WeldGood
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedExcellent
Forgeability Rating65
Machinability Rating30
Common Fabrication Processes
  • Forming and Bending
  • Heading and Upsetting
  • Hot Forging and Pressing
  • Roll Threading and Knurling
  • Shearing
  • Swaging
    
Thermal Properties
Treatment Minimum* Maximum* Value*
* Temperature is measured in Fahrenheit.
Solution Treatment13001450
Precipitation Treatment850
Annealing9001300
Hot Treatment13001550
Typical uses
Product Category Product Reason Category Reason
ElectricalConnectorsConductivity (Electrical)Electrical Conductivity
ConnectorsConductivity (Thermal)Thermal Conductivity
ConnectorsCorrosion ResistanceCorrosion Resistance
ConnectorsMechanical PropertiesHigh Strength
ConnectorsSolderabilitySolderability
Electronic Parts for Electron Tube ComponentsConductivity (Electrical)Electrical Conductivity
Electronic Parts for Electron Tube ComponentsConductivity (Thermal)Thermal Conductivity
Electronic Parts for Electron Tube ComponentsCorrosion ResistanceCorrosion Resistance
Electronic Parts for Electron Tube ComponentsSolderabilitySolderability
Electronic Parts for Power Tube ComponentsConductivity (Electrical)Electrical Conductivity
Electronic Parts for Power Tube ComponentsConductivity (Thermal)Thermal Conductivity
Electronic Parts for Power Tube ComponentsCorrosion ResistanceCorrosion Resistance
Electronic Parts for Power Tube ComponentsSolderabilitySolderability
High Strength Electrical ConductorsConductivity (Electrical)Electrical Conductivity
High Strength Electrical ConductorsConductivity (Thermal)Thermal Conductivity
High Strength Electrical ConductorsCorrosion ResistanceCorrosion Resistance
High Strength Electrical ConductorsMechanical PropertiesHigh Strength
FastenersBoltsCorrosion ResistanceCorrosion Resistance
BoltsMechanical PropertiesHigh Strength
ClipsCorrosion ResistanceCorrosion Resistance
ClipsMechanical PropertiesFatigue Resistance
ClipsMechanical PropertiesHigh Strength
Cotter PinsCorrosion ResistanceCorrosion Resistance
Cotter PinsMechanical PropertiesHigh Strength
NailsCorrosion ResistanceCorrosion Resistance
NailsMechanical PropertiesHigh Strength
ScrewsCorrosion ResistanceCorrosion Resistance
ScrewsMechanical PropertiesHigh Strength
IndustrialSpringsCorrosion ResistanceCorrosion Resistance
SpringsMechanical PropertiesFatigue Resistance
SpringsMechanical PropertiesHigh Strength
Applicable Specifications

No applicable specifications for this alloy

Corrosion Properties

No information available.