Find suppliers for this alloyC19024
Chemical Composition
Element
Cu(1,2)PbSnZnFePNi
(1) Cu + Sum of Named Elements 99.9% min. (2) Cu value includes Ag.
Min (%).020.0080.10
Max (%)Rem0.010.80.050.020.050.6
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.2% Offset
Elongation
(%)
Vickers Hardness, 500 gm
Flat Products1/2 HardH0248   Min
58   Max
40.5   Min
8   Min
90   Min
110   Max
Extra HardH0664   Min
72.5   Max
58   Min
4   Min
120   Min
145   Max
HardH0455   Min
67   Max
51.5   Min
5   Min
115   Min
135   Max
SpringH0869.5   Min
65   Min
2   Min
140   Min
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1976
Melting Point - Solidus°F1958
Densitylb/cu in. at 68°F0.322
Specific Gravity8.9
Electrical Conductivity% IACS at 68°F62
Modulus of Elasticity in Tensionksi18250
Modulus of Rigidityksi6800
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingGood
Fabrication Process Properties

No fabrication process properties for this alloy

    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Solution Treatment392572
Annealing9321112
Hot Treatment12921562
Typical uses
Product Category Product Reason Category Reason
ElectricalSprings, connectors, terminals, leads
Applicable Specifications

No applicable specifications for this alloy

Corrosion Properties

No information available.