Find suppliers for this alloy
C19027
| Elements | |||||||
|---|---|---|---|---|---|---|---|
| Cu(1,2) | Sn | Zn | Fe | P | Ni | Mg | |
|
(1) Cu + Sum of Named Elements 99.7% min. (2) Cu value includes Ag. |
|||||||
| Min (%) | 1.20 | 0.03 | 0.50 | ||||
| Max (%) | Rem | 1.80 | 0.20 | 0.10 | 0.15 | 1.20 | 0.20 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Vickers Hardness, 500 gm |
|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||
| Flat Products | 1/2 Hard | H02 |
73 Min 77 Typ 893 Max |
70 Min 76 Typ 82 Max |
5 Min 10 Typ 14 Max |
155 Min 165 Typ 180 Max |
| Extra Hard | H06 |
84 Min 90 Typ 96 Max |
81 Min 87 Typ 94 Max |
3 Min 7 Typ 10 Max |
180 Min 205 Typ 215 Max |
|
| Hard | H04 |
78 Min 83 Typ 90 Max |
77 Min 82 Typ 89 Max |
4 Min 9 Typ 12 Max |
160 Min 175 Typ 195 Max |
|
| Spring | H08 |
91 Min 97 Typ 106 Max |
88 Min 91 Typ 105 Max |
5 Typ |
190 Min 210 Typ |
|
| Melting Point - Liquidus°F | 1976 |
|---|---|
| Densitylb/cu in. at 68°F | 0.321 |
| Specific Gravity | 8.9 |
| Electrical Conductivity% IACS at 68°F | 30 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 80 |
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 9.4 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 19000 |
| Modulus of Rigidityksi | 6200 |
Fabrication Properties
Common Fabrication Processes
Thermal Properties
Typical Uses
Applicable Specifications
Corrosion Properties