C19100
| Elements | |||||||
|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Zn | Fe | P | Ni | Te | |
|
(1) Cu + Sum of Named Elements 99.5% min. (2) Cu value includes Ag. |
|||||||
| Min (%) | 0.15 | 0.9 | 0.35 | ||||
| Max (%) | Rem | 0.10 | 0.50 | 0.20 | 0.35 | 1.3 | 0.6 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Rockwell F scale | Shear Strength (ksi) |
Fatigue Strength** (ksi) |
Section Size (in) |
Cold Work (%) |
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | ||||||||||||
| Forgings | As Forged - Quenched | M11 |
36 Typ |
10 Typ |
35 Typ |
|||||||
| As Hot Forged - Air Cooled | M10 |
45 Typ |
12 Typ |
50 Typ |
||||||||
| Precipitation Hardened | TF00 |
58 Typ |
38 Typ |
70 Typ |
97 Typ |
|||||||
| Rod | 1/4 Hard and Stress Relieved | HR01 |
78 Typ |
70 Typ |
68 Typ |
27 Typ |
84 Typ |
41 Typ |
33 Typ | 1 | ||
| 1/4 Hard and Stress Relieved | HR01 |
104 Typ |
92 Typ |
77 Typ |
6 Typ |
95 Typ |
56 Typ |
0.125 | 75 | |||
| 1/4 Hard and Stress Relieved | HR01 |
84 Typ |
77 Typ |
73 Typ |
10 Typ |
85 Typ |
44 Typ |
33 Typ | 0.25 | 35 | ||
| 1/4 Hard and Stress Relieved | HR01 |
80 Typ |
73 Typ |
70 Typ |
15 Typ |
85 Typ |
43 Typ |
0.5 | ||||
| 1/4 Hard and Stress Relieved | HR01 |
94 Typ |
86 Typ |
75 Typ |
10 Typ |
90 Typ |
48 Typ |
0.375 | ||||
| (1)Precipitation heat treated. | |
| Melting Point - Liquidus°F | 1980 |
|---|---|
| Melting Point - Solidus°F | 1900 |
| Densitylb/cu in. at 68°F | 0.323 |
| Specific Gravity | 8.94 |
| Electrical Conductivity% IACS at 68°F | 55 (1) |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 145 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.8 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.092 |
| Modulus of Elasticity in Tensionksi | 16000 |
| Modulus of Rigidityksi | 6000 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Good |
| Oxyacetylene Welding | Fair |
| Gas Shielded Arc Welding | Fair |
| Coated Metal Arc Welding | Fair |
| Spot Weld | Poor |
| Seam Weld | Poor |
| Butt Weld | Poor |
| Capacity for Being Cold Worked | Good |
| Capacity for Being Hot Formed | Good |
| Forgeability Rating | 65 |
| Machinability Rating | 75 |
Common Fabrication Processes
- Forming and Bending
- Heading and Upsetting
- Hot Forging and Pressing
- Machining
- Roll Threading and Knurling
- Shearing
- Swaging
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 900 | 1300 | ||
| Hot Working Temperature | 1400 | 1600 | ||
| Precipitation Treatment | 850 | |||
| Solution Treatment | 1300 | 1450 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Electrical | Components | Conductivity (Electrical) | Electrical Conductivity |
| Components | Conductivity (Thermal) | Thermal Conductivity | |
| Components | Corrosion Resistance | Corrosion Resistance | |
| Components | Mechanical Properties | High Strength | |
| Connectors | Conductivity (Electrical) | Electrical Conductivity | |
| Connectors | Conductivity (Thermal) | Thermal Conductivity | |
| Connectors | Corrosion Resistance | Corrosion Resistance | |
| Connectors | Mechanical Properties | High Strength | |
| Connectors | Solderability | Solderability | |
| Fasteners | Bolts | Corrosion Resistance | Corrosion Resistance |
| Bolts | Machining Characteristics | Machinability | |
| Bolts | Mechanical Properties | High Strength | |
| Nuts | Corrosion Resistance | Corrosion Resistance | |
| Nuts | Forming Characteristics | Formability | |
| Nuts | Machining Characteristics | Machinability | |
| Nuts | Mechanical Properties | High Strength | |
| Turn buckle Barrels | Corrosion Resistance | Corrosion Resistance | |
| Turn buckle Barrels | Machining Characteristics | Machinability | |
| Turn buckle Barrels | Mechanical Properties | High Strength | |
| Industrial | Bushings | Corrosion Resistance | Corrosion Resistance |
| Bushings | Friction & Wear Properties | Wear Resistance | |
| Bushings | Machining Characteristics | Machinability | |
| Bushings | Mechanical Properties | High Strength | |
| Forgings | Corrosion Resistance | Corrosion Resistance | |
| Forgings | Forming Characteristics | Formability | |
| Forgings | Machining Characteristics | Machinability | |
| Forgings | Mechanical Properties | Fatigue Resistance | |
| Forgings | Mechanical Properties | High Strength | |
| Gears | Corrosion Resistance | Corrosion Resistance | |
| Gears | Machining Characteristics | Machinability | |
| Gears | Mechanical Properties | High Strength | |
| Pinions | Corrosion Resistance | Corrosion Resistance | |
| Pinions | Machining Characteristics | Machinability | |
| Pinions | Mechanical Properties | High Strength | |
| Screw Machine Parts | Corrosion Resistance | Corrosion Resistance | |
| Screw Machine Parts | Machining Characteristics | Machinability | |
| Screw Machine Parts | Mechanical Properties | High Strength | |
| Tie Rods | Corrosion Resistance | Corrosion Resistance | |
| Tie Rods | Machining Characteristics | Machinability | |
| Tie Rods | Mechanical Properties | High Strength | |
| Welding Torch Tips | Conductivity (Thermal) | Thermal Conductivity | |
| Welding Torch Tips | Corrosion Resistance | Corrosion Resistance | |
| Welding Torch Tips | Mechanical Properties | High Strength | |
| Marine | Hardware | Corrosion Resistance | Corrosion Resistance |
| Hardware | Machining Characteristics | Machinability | |
| Hardware | Mechanical Properties | High Strength |
Applicable Specifications
Corrosion Properties