Find suppliers for this alloyC19160
Chemical Composition
Element
Cu(1,2)PbSnZnFePNi
(1) Cu value includes Ag. (2) Cu + Sum of Named Elements 99.5% min.
Min (%)0.80.150.8
Max (%)Rem1.20.050.500.050.351.2
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Section Size
(in)
RodPrecipitation Heat Treated or Spinodal Heat Treated and HardTL0485   Typ
75   Typ
5   Typ
0.078
WirePrecipitation HardenedTF0065   Typ
40   Typ
25   Typ
0.08
Precipitation Heat Treated or Spinodal Heat Treated and 1/2 HardTL0286   Typ
70   Typ
7   Typ
0.08
Precipitation Heat Treated or Spinodal Heat Treated and 1/4 HardTL0178.5   Typ
68   Typ
12   Typ
0.08
Precipitation Heat Treated or Spinodal Heat Treated and HardTL0495   Typ
75   Typ
5   Typ
0.08
Precipitation Heat Treated or Spinodal Heat Treated and SpringTL08107   Typ
98   Typ
3   Typ
0.08
* Measured at room temperature, 68°F (20°C).
Physical Properties
(1) Volume basis, after aging treatment
(2) After aging treatment
Melting Point - Liquidus°F1980
Melting Point - Solidus°F1900
Densitylb/cu in. at 68°F0.32
Specific Gravity8.88
Electrical Conductivity% IACS at 68°F55(1)
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F146(2)
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)9.8
Specific Heat CapacityBtu/ lb /°F at 68°F0.092
Modulus of Elasticity in Tensionksi18000
Modulus of Rigidityksi6000
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingGood
Oxyacetylene WeldingNot Recommended
Gas Shielded Arc WeldingNot Recommended
Coated Metal Arc WeldingNot Recommended
Spot WeldNot Recommended
Seam WeldNot Recommended
Butt WeldFair
Capacity for Being Cold WorkedGood
Capacity for Being Hot FormedPoor
Machinability Rating80
Common Fabrication Processes
  • Cold Heading
  • Machining
    
Thermal Properties
Treatment Minimum* Maximum* Value*
* Temperature is measured in Fahrenheit.
Solution Treatment13001450
Precipitation Treatment800
Hot Treatment14001600
Typical uses
Product Category Product Reason Category Reason
ElectricalConnector Pins
ContactsConductivity (Electrical)Electrical Conductivity
ContactsConductivity (Thermal)Thermal Conductivity
ContactsCorrosion ResistanceCorrosion Resistance
ContactsMechanical PropertiesModerate Strength
ContactsSolderabilitySolderability
SocketsConductivity (Electrical)Electrical Conductivity
SocketsConductivity (Thermal)Thermal Conductivity
SocketsCorrosion ResistanceCorrosion Resistance
SocketsMechanical PropertiesHigh Strength
Applicable Specifications

No applicable specifications for this alloy

Corrosion Properties

No information available.