Find suppliers for this alloy
C19200
| Elements | ||||
|---|---|---|---|---|
| Cu(1) | Zn | Fe | P | |
|
(1) Cu + Sum of Named Elements 99.8% min. |
||||
| Min (%) | 98.5 | 0.8 | 0.01 | |
| Max (%) | 0.20 | 1.2 | 0.04 | |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Torsion Modulus (ksi) |
Section Size (in) |
Cold Work (%) |
|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||||||
| Flat Products | 1/2 Hard | H02 |
65 Typ |
45 Typ |
18 Typ |
55 Typ |
0.04 | |||
| 1/4 Hard | H01 |
50 Typ |
37 Typ |
25 Typ |
45 Typ |
0.04 | ||||
| Extra Hard | H06 |
70 Typ |
66 Typ |
3 Typ |
75 Typ |
0.04 | ||||
| Extra Spring | H10 |
77 Typ |
74 Typ |
2 Typ |
77 Typ |
0.04 | ||||
| Hard | H04 |
65 Typ |
60 Typ |
7 Typ |
72 Typ |
6.4 Typ | 0.04 | |||
| Light Drawn, Light Cold Rolled | H55 |
42 Typ |
30 Typ |
31 Typ |
35 Typ |
|||||
| Soft Anneal | O60 |
45 Typ |
20 Typ |
25 Typ |
38 Typ |
|||||
| Spring | H08 |
74 Typ |
71 Typ |
2 Typ |
76 Typ |
0.04 | ||||
| Tube | Hard Drawn | H80 |
56 Typ |
52 Typ |
52 Typ |
7 Typ |
40 | |||
| Light Anneal | O50 |
42 Typ |
22 Typ |
23 Typ |
30 Typ |
|||||
| Light Drawn, Light Cold Rolled | H55 |
42 Typ |
30 Typ |
35 Typ |
||||||
| Soft Anneal | O60 |
37 Typ |
11 Typ |
12 Typ |
40 Typ |
|||||
| (1)Applies only to tube.(2)Applies only to strip.(3)Applies only to tube.(4)Applies only to strip. | |
| Melting Point - Liquidus°F | 1983 |
|---|---|
| Melting Point - Solidus°F | 1973 |
| Densitylb/cu in. at 68°F | 0.32 |
| Specific Gravity | 8.87 |
| Electrical Conductivity% IACS at 68°F | 50 (1) |
| Electrical Conductivity% IACS at 68°F | 65 (2) |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 125 (3) |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 150 (4) |
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 9 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 17000 |
| Modulus of Rigidityksi | 6400 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Good |
| Gas Shielded Arc Welding | Excellent |
| Coated Metal Arc Welding | Not Recommended |
| Spot Weld | Not Recommended |
| Seam Weld | Not Recommended |
| Butt Weld | Good |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Excellent |
| Forgeability Rating | 65 |
| Machinability Rating | 20 |
Common Fabrication Processes
- Blanking
- Coining
- Coppersmithing
- Drawing
- Etching
- Forming and Bending
- Heading and Upsetting
- Hot Forging and Pressing
- Piercing and Punching
- Roll Threading and Knurling
- Shearing
- Spinning
- Squeezing and Swaging
- Stamping
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 1300 | 1500 | ||
| Hot Working Temperature | 1500 | 1750 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Automotive | Hydraulic Brake Lines | Corrosion Resistance | Corrosion Resistance |
| Hydraulic Brake Lines | Corrosion Resistance | Stress Corrosion Cracking Resistance | |
| Hydraulic Brake Lines | Mechanical Properties | Moderate Strength | |
| Hydraulic Brake Lines | Welding Characteristics | Weldability | |
| Consumer | Gift Hollow Ware | Appearance | Appearance |
| Gift Hollow Ware | Corrosion Resistance | Corrosion Resistance | |
| Gift Hollow Ware | Forming Characteristics | Formability | |
| Gift Hollow Ware | Mechanical Properties | Moderate Strength | |
| Electrical | Cable Wrap | Conductivity (Electrical) | Electrical Conductivity |
| Cable Wrap | Conductivity (Thermal) | Thermal Conductivity | |
| Cable Wrap | Corrosion Resistance | Corrosion Resistance | |
| Cable Wrap | Forming Characteristics | Formability | |
| Cable Wrap | Mechanical Properties | Moderate Strength | |
| Cable Wrap | Softening Resistance | Resistance to Thermal Softening | |
| Circuit Breaker Parts | Conductivity (Electrical) | Electrical Conductivity | |
| Circuit Breaker Parts | Conductivity (Thermal) | Thermal Conductivity | |
| Circuit Breaker Parts | Corrosion Resistance | Corrosion Resistance | |
| Circuit Breaker Parts | Mechanical Properties | Moderate Strength | |
| Circuit Breaker Parts | Softening Resistance | Resistance to Thermal Softening | |
| Connectors | Conductivity (Electrical) | Electrical Conductivity | |
| Connectors | Conductivity (Thermal) | Thermal Conductivity | |
| Connectors | Corrosion Resistance | Corrosion Resistance | |
| Connectors | Mechanical Properties | Moderate Strength | |
| Contact springs | Conductivity (Electrical) | Electrical Conductivity | |
| Contact springs | Conductivity (Thermal) | Thermal Conductivity | |
| Contact springs | Corrosion Resistance | Corrosion Resistance | |
| Contact springs | Forming Characteristics | Formability | |
| Contact springs | Mechanical Properties | Moderate Strength | |
| Fuse Clips | Conductivity (Electrical) | Electrical Conductivity | |
| Fuse Clips | Conductivity (Thermal) | Thermal Conductivity | |
| Fuse Clips | Corrosion Resistance | Corrosion Resistance | |
| Fuse Clips | Forming Characteristics | Formability | |
| Fuse Clips | Mechanical Properties | Moderate Strength | |
| Lead Frames | Conductivity (Electrical) | Electrical Conductivity | |
| Lead Frames | Conductivity (Thermal) | Thermal Conductivity | |
| Lead Frames | Corrosion Resistance | Corrosion Resistance | |
| Lead Frames | Forming Characteristics | Formability | |
| Lead Frames | Mechanical Properties | Moderate Strength | |
| Lead Frames | Solderability | Solderability | |
| Terminals | Conductivity (Electrical) | Electrical Conductivity | |
| Terminals | Conductivity (Thermal) | Thermal Conductivity | |
| Terminals | Corrosion Resistance | Corrosion Resistance | |
| Terminals | Forming Characteristics | Formability | |
| Terminals | Mechanical Properties | High Strength | |
| Fasteners | Eyelets | Appearance | Appearance |
| Eyelets | Corrosion Resistance | Corrosion Resistance | |
| Eyelets | Forming Characteristics | Formability | |
| Eyelets | Mechanical Properties | Moderate Strength | |
| Industrial | Flexible Hose | Corrosion Resistance | Corrosion Resistance |
| Flexible Hose | Mechanical Properties | Moderate Strength | |
| Flexible Hose | Solderability | Solderability | |
| Flexible Hose | Welding Characteristics | Weldability | |
| Gaskets | Corrosion Resistance | Corrosion Resistance | |
| Gaskets | Forming Characteristics | Formability | |
| Gaskets | Mechanical Properties | Moderate Strength | |
| Heat Exchanger Tubing | Conductivity (Thermal) | Thermal Conductivity | |
| Heat Exchanger Tubing | Corrosion Resistance | Corrosion Resistance | |
| Heat Exchanger Tubing | Mechanical Properties | Moderate Strength | |
| Heat Exchanger Tubing | Softening Resistance | Resistance to Thermal Softening | |
| Heat Exchanger Tubing | Welding Characteristics | Weldability | |
| Plumbing | Air Conditioning Tubing | Corrosion Resistance | Corrosion Resistance |
| Air Conditioning Tubing | Forming Characteristics | Formability | |
| Air Conditioning Tubing | Mechanical Properties | Moderate Strength | |
| Air Conditioning Tubing | Solderability | Solderability | |
| Air Conditioning Tubing | Welding Characteristics | Weldability |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Bar | ASTM | B465 | COPPER-IRON ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR | ||
| Condenser & Heat Exchanger Tube with Integral Fins | ASTM | B956/B956M | WELDED COPPER AND COPPER-ALLOY CONDENSER AND HEAT EXCHANGER TUBES WITH INTEGRAL FINS | ||
| Plate | ASTM | B465 | COPPER-IRON ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR | ||
| Seamless Condenser Tube & Ferrule Stock | Condenser Tube | ASTM | B111/B111M | COPPER AND COPPER ALLOY SEAMLESS CONDENSER TUBES AND FERRULE STOCK | |
| Seamless Heat Exchanger Tube with Integral Fins | ASME | SB359 | COPPER & COPPER ALLOY SEAMLESS CONDENSER & HEAT EXCHANGER TUBES WITH INTEGRAL FINS | ||
| Seamless Heat Exchanger and Condenser Tube | ASME | SB395 | U-BEND SEAMLESS COPPER & COPPER ALLOY HEAT EXCHANGER & CONDENSER TUBE | ||
| Sheet | ASTM | B465 | COPPER-IRON ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR | ||
| Strip | ASTM | B465 | COPPER-IRON ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR | ||
| Tube | Condenser Tube | ASME | SB111 | COPPER AND COPPER ALLOY SEAMLESS CONDENSER TUBES & FERRULE STOCK | |
| SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |||
| SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | |||
| ASTM | B469 | SEAMLESS COPPER ALLOY TUBES FOR PRESSURE APPLICATION | |||
| Tube, Condenser & Heat Exchanger, Seamless w/ Fins | ASTM | B359/B359M | COPPER AND COPPER-ALLOY SEAMLESS CONDENSER AND HEAT EXCHANGER TUBES WITH INTEGRAL FINS | ||
| Tubes, Seamless Condenser & Heat Exchanger, U-Bend | ASTM | B395/B395M | U-BEND SEAMLESS COPPER AND COPPER ALLOY HEAT EXCHANGER AND CONDENSER TUBES | ||
| Welded Heat Exchanger & Condenser Tube | with Integral Fins | ASME | SB956 | Tube, Welded, Condenser, Heat Exchanger, w/ Integral Fins |
Corrosion Properties