Find suppliers for this alloyC19200
Chemical Composition
Element
Cu(1)ZnFeP
(1) Cu + Sum of Named Elements 99.8% min.
Min (%)98.50.80.01
Max (%)0.201.20.04
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.2% Offset
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Torsion Modulus
(ksi)
Section Size
(in)
Cold Work
(%)
Flat Products1/2 HardH0265   Typ
45   Typ
18   Typ
55   Typ
0.04
1/4 HardH0150   Typ
37   Typ
25   Typ
45   Typ
0.04
Extra HardH0670   Typ
66   Typ
3   Typ
75   Typ
0.04
Extra SpringH1077   Typ
74   Typ
2   Typ
77   Typ
0.04
HardH0465   Typ
60   Typ
7   Typ
72   Typ
6.4   Typ
0.04
Light Drawn, Light Cold RolledH5542   Typ
30   Typ
31   Typ
35   Typ
Soft AnnealO6045   Typ
20   Typ
25   Typ
38   Typ
SpringH0874   Typ
71   Typ
2   Typ
76   Typ
0.04
TubeHard DrawnH8056   Typ
52   Typ
52   Typ
7   Typ
40
Light AnnealO5042   Typ
22   Typ
23   Typ
30   Typ
Light Drawn, Light Cold RolledH5542   Typ
30   Typ
35   Typ
Soft AnnealO6037   Typ
11   Typ
12   Typ
40   Typ
* Measured at room temperature, 68°F (20°C).
Physical Properties
(1) Applies only to tube.
(2) Applies only to strip.
(3) Applies only to tube.
(4) Applies only to strip.
Melting Point - Liquidus°F1983
Melting Point - Solidus°F1973
Densitylb/cu in. at 68°F0.32
Specific Gravity8.87
Electrical Conductivity% IACS at 68°F50(1)
Electrical Conductivity% IACS at 68°F65(2)
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F125(3)
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F150(4)
Coefficient of Thermal Expansion 68-21210⁻⁶ per °F (68 – 212°F)9
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi17000
Modulus of Rigidityksi6400
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingGood
Gas Shielded Arc WeldingExcellent
Coated Metal Arc WeldingNot Recommended
Spot WeldNot Recommended
Seam WeldNot Recommended
Butt WeldGood
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedExcellent
Forgeability Rating65
Machinability Rating20
Common Fabrication Processes
  • Blanking
  • Coining
  • Coppersmithing
  • Drawing
  • Etching
  • Forming and Bending
  • Heading and Upsetting
  • Hot Forging and Pressing
  • Piercing and Punching
  • Roll Threading and Knurling
  • Shearing
  • Spinning
  • Squeezing and Swaging
  • Stamping
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing13001500
Hot Treatment15001750
Typical uses
Product Category Product Reason Category Reason
AutomotiveHydraulic Brake LinesCorrosion ResistanceCorrosion Resistance
Hydraulic Brake LinesCorrosion ResistanceStress Corrosion Cracking Resistance
Hydraulic Brake LinesMechanical PropertiesModerate Strength
Hydraulic Brake LinesWelding CharacteristicsWeldability
ConsumerGift Hollow WareAppearanceAppearance
Gift Hollow WareCorrosion ResistanceCorrosion Resistance
Gift Hollow WareForming CharacteristicsFormability
Gift Hollow WareMechanical PropertiesModerate Strength
ElectricalCable WrapConductivity (Electrical)Electrical Conductivity
Cable WrapConductivity (Thermal)Thermal Conductivity
Cable WrapCorrosion ResistanceCorrosion Resistance
Cable WrapForming CharacteristicsFormability
Cable WrapMechanical PropertiesModerate Strength
Cable WrapSoftening ResistanceResistance to Thermal Softening
Circuit Breaker PartsConductivity (Electrical)Electrical Conductivity
Circuit Breaker PartsConductivity (Thermal)Thermal Conductivity
Circuit Breaker PartsCorrosion ResistanceCorrosion Resistance
Circuit Breaker PartsMechanical PropertiesModerate Strength
Circuit Breaker PartsSoftening ResistanceResistance to Thermal Softening
ConnectorsConductivity (Electrical)Electrical Conductivity
ConnectorsConductivity (Thermal)Thermal Conductivity
ConnectorsCorrosion ResistanceCorrosion Resistance
ConnectorsMechanical PropertiesModerate Strength
Contact springsConductivity (Electrical)Electrical Conductivity
Contact springsConductivity (Thermal)Thermal Conductivity
Contact springsCorrosion ResistanceCorrosion Resistance
Contact springsForming CharacteristicsFormability
Contact springsMechanical PropertiesModerate Strength
Fuse ClipsConductivity (Electrical)Electrical Conductivity
Fuse ClipsConductivity (Thermal)Thermal Conductivity
Fuse ClipsCorrosion ResistanceCorrosion Resistance
Fuse ClipsForming CharacteristicsFormability
Fuse ClipsMechanical PropertiesModerate Strength
Lead FramesConductivity (Electrical)Electrical Conductivity
Lead FramesConductivity (Thermal)Thermal Conductivity
Lead FramesCorrosion ResistanceCorrosion Resistance
Lead FramesForming CharacteristicsFormability
Lead FramesMechanical PropertiesModerate Strength
Lead FramesSolderabilitySolderability
TerminalsConductivity (Electrical)Electrical Conductivity
TerminalsConductivity (Thermal)Thermal Conductivity
TerminalsCorrosion ResistanceCorrosion Resistance
TerminalsForming CharacteristicsFormability
TerminalsMechanical PropertiesHigh Strength
FastenersEyeletsAppearanceAppearance
EyeletsCorrosion ResistanceCorrosion Resistance
EyeletsForming CharacteristicsFormability
EyeletsMechanical PropertiesModerate Strength
IndustrialFlexible HoseCorrosion ResistanceCorrosion Resistance
Flexible HoseMechanical PropertiesModerate Strength
Flexible HoseSolderabilitySolderability
Flexible HoseWelding CharacteristicsWeldability
GasketsCorrosion ResistanceCorrosion Resistance
GasketsForming CharacteristicsFormability
GasketsMechanical PropertiesModerate Strength
Heat Exchanger TubingConductivity (Thermal)Thermal Conductivity
Heat Exchanger TubingCorrosion ResistanceCorrosion Resistance
Heat Exchanger TubingMechanical PropertiesModerate Strength
Heat Exchanger TubingSoftening ResistanceResistance to Thermal Softening
Heat Exchanger TubingWelding CharacteristicsWeldability
PlumbingAir Conditioning TubingCorrosion ResistanceCorrosion Resistance
Air Conditioning TubingForming CharacteristicsFormability
Air Conditioning TubingMechanical PropertiesModerate Strength
Air Conditioning TubingSolderabilitySolderability
Air Conditioning TubingWelding CharacteristicsWeldability
Applicable Specifications
Form Sub-Form Specific Sub-Form Application System Standard Description
BarASTMB465COPPER-IRON ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
Condenser & Heat Exchanger Tube with Integral FinsWeldedASTMB956/B956MWELDED COPPER AND COPPER-ALLOY CONDENSER AND HEAT EXCHANGER TUBES WITH INTEGRAL FINS
PlateASTMB465COPPER-IRON ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
Seamless Condenser Tube & Ferrule StockCondenser TubeASTMB111/B111MCOPPER AND COPPER ALLOY SEAMLESS CONDENSER TUBES AND FERRULE STOCK
Seamless Heat Exchanger and Condenser TubeU-BendASMESB395U-BEND SEAMLESS COPPER & COPPER ALLOY HEAT EXCHANGER & CONDENSER TUBE
Seamless Heat Exchanger Tube with Integral FinsFinnedASMESB359COPPER & COPPER ALLOY SEAMLESS CONDENSER & HEAT EXCHANGER TUBES WITH INTEGRAL FINS
SheetASTMB465COPPER-IRON ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
StripASTMB465COPPER-IRON ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
TubeCondenser TubeASMESB111COPPER AND COPPER ALLOY SEAMLESS CONDENSER TUBES & FERRULE STOCK
SeamlessASTMB469SEAMLESS COPPER ALLOY TUBES FOR PRESSURE APPLICATION
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
Tube, Condenser & Heat Exchanger, Seamless w/ FinsFinnedASTMB359/B359MCOPPER AND COPPER-ALLOY SEAMLESS CONDENSER AND HEAT EXCHANGER TUBES WITH INTEGRAL FINS
Tubes, Seamless Condenser & Heat Exchanger, U-BendU-BendASTMB395/B395MU-BEND SEAMLESS COPPER AND COPPER ALLOY HEAT EXCHANGER AND CONDENSER TUBES
Welded Heat Exchanger & Condenser Tubewith Integral FinsASMESB956Tube, Welded, Condenser, Heat Exchanger, w/ Integral Fins
Corrosion Properties

No information available.