C19210
| Elements | |||
|---|---|---|---|
| Cu(1) | Fe | P | |
|
(1) Cu + Sum of Named Elements 99.8% min. |
|||
| Min (%) | 0.05 | 0.025 | |
| Max (%) | Rem | 0.15 | 0.04 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Section Size (in) |
|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||
| Sheet | 1/2 Hard | H02 |
57 Typ |
56 Typ |
6 Typ |
0.018 |
| 1/4 Hard | H01 |
50 Typ |
48 Typ |
13 Typ |
0.018 | |
| Hard | H04 |
64 Typ |
63 Typ |
3.5 Typ |
0.018 | |
| Light Anneal | O50 |
43 Typ |
22 Typ |
38 Typ |
0.018 | |
| Spring | H08 |
71 Typ |
70 Typ |
2 Typ |
0.018 | |
| Melting Point - Liquidus°F | 1980 |
|---|---|
| Densitylb/cu in. at 68°F | 0.323 |
| Specific Gravity | 8.94 |
| Electrical Conductivity% IACS at 68°F | 80 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.4 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.092 |
| Modulus of Elasticity in Tensionksi | 18200 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Good |
| Gas Shielded Arc Welding | Not Recommended |
| Coated Metal Arc Welding | Excellent |
| Spot Weld | Not Recommended |
| Seam Weld | Not Recommended |
| Butt Weld | Good |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Excellent |
| Forgeability Rating | 65 |
| Machinability Rating | 20 |
Common Fabrication Processes
- Forming and Bending
- Heading and Upsetting
- Piercing and Punching
- Shearing
- Spinning
- Squeezing and Swaging
- Stamping
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 840 | 1020 | ||
| Hot Working Temperature | 1300 | 1650 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Automotive | Cooling Fins for Radiators | Conductivity (Thermal) | Thermal Conductivity |
| Cooling Fins for Radiators | Corrosion Resistance | Corrosion Resistance | |
| Cooling Fins for Radiators | Forming Characteristics | Formability | |
| Cooling Fins for Radiators | Mechanical Properties | Moderate Strength | |
| Building | Air Conditioning Tubing | Corrosion Resistance | Corrosion Resistance |
| Air Conditioning Tubing | Mechanical Properties | Moderate Strength | |
| Air Conditioning Tubing | Solderability | Solderability | |
| Air Conditioning Tubing | Welding Characteristics | Weldability | |
| Electrical | Connectors | Conductivity (Electrical) | Electrical Conductivity |
| Connectors | Conductivity (Thermal) | Thermal Conductivity | |
| Connectors | Corrosion Resistance | Corrosion Resistance | |
| Connectors | Mechanical Properties | Moderate Strength | |
| IC Lead Frames | Conductivity (Electrical) | Electrical Conductivity | |
| IC Lead Frames | Conductivity (Thermal) | Thermal Conductivity | |
| IC Lead Frames | Corrosion Resistance | Corrosion Resistance | |
| IC Lead Frames | Forming Characteristics | Formability | |
| IC Lead Frames | Mechanical Properties | Moderate Strength | |
| IC Lead Frames | Solderability | Solderability | |
| Terminals | Conductivity (Electrical) | Electrical Conductivity | |
| Terminals | Conductivity (Thermal) | Thermal Conductivity | |
| Terminals | Corrosion Resistance | Corrosion Resistance | |
| Terminals | Forming Characteristics | Formability | |
| Terminals | Mechanical Properties | Moderate Strength | |
| Terminals | Solderability | Solderability | |
| Industrial | Cooling Fins for Heavy Duty Radiators | Conductivity (Thermal) | Thermal Conductivity |
| Cooling Fins for Heavy Duty Radiators | Corrosion Resistance | Corrosion Resistance | |
| Cooling Fins for Heavy Duty Radiators | Forming Characteristics | Formability | |
| Cooling Fins for Heavy Duty Radiators | Mechanical Properties | Moderate Strength | |
| Cooling Fins for Heavy Duty Radiators | Softening Resistance | Resistance to Thermal Softening | |
| Heat Exchanger Tubing | Appearance | Appearance | |
| Heat Exchanger Tubing | Conductivity (Thermal) | Thermal Conductivity | |
| Heat Exchanger Tubing | Corrosion Resistance | Corrosion Resistance | |
| Heat Exchanger Tubing | Forming Characteristics | Formability | |
| Heat Exchanger Tubing | Mechanical Properties | Moderate Strength | |
| Heat Resistant Applications | Conductivity (Thermal) | Thermal Conductivity | |
| Heat Resistant Applications | Corrosion Resistance | Corrosion Resistance | |
| Heat Resistant Applications | Forming Characteristics | Formability | |
| Heat Resistant Applications | Mechanical Properties | Moderate Strength |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Strip | ASTM | B888/B88M | COPPER ALLOY STRIP FOR USE IN MANUFACTURE OF ELECTRICAL CONNECTORS OR SPRING CONTACTS | ||
| Strip, Sheet & Plate | ASTM | B465 | COPPER-IRON ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR |
Corrosion Properties