Chemical Composition
Element
CuPbZnFeP
Min (%)97.00.052.10.015
Max (%)0.030.202.60.15
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.2% Offset
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell 30T scale
Fatigue Strength**
(ksi)
Section Size
(in)
Cold Work
(%)
Flat Products1/2 HardH0260   Typ
53   Typ
50   Typ
9   Typ
68   Typ
66   Typ
0.04
Extra HardH0670   Typ
68   Typ
3   Typ
74   Typ
71   Typ
0.04
Extra SpringH1076   Typ
73   Typ
2   Typ
77   Typ
74   Typ
21   Typ
0.04
HardH0467   Typ
63   Typ
4   Typ
73   Typ
69   Typ
21   Typ
0.04
Light AnnealO5050   Typ
30   Typ
29   Typ
45   Typ
0.025
Soft AnnealO6045   Typ
24   Typ
32   Typ
38   Typ
16   Typ
0.025
SpringH0873   Typ
71   Typ
2   Typ
75   Typ
72   Typ
22   Typ
0.04
Super SpringH1480   Typ
73   Min
1   Typ
73   Min
0.04
Tube1/2 HardH0258   Typ
55   Typ
9   Typ
61   Typ
60   Typ
0.035
As-Welded from Extra Spring StripWM1076   Typ
73   Typ
1   Typ
76   Typ
69   Typ
0.035
As-Welded from Hard StripWM0465   Typ
63   Typ
4   Typ
73   Typ
66   Typ
0.035
Hard DrawnH8068   Typ
66   Typ
2   Typ
73   Typ
66   Typ
0.03535
Light AnnealO5050   Typ
30   Typ
16   Typ
45   Typ
0.035
Soft AnnealO6045   Typ
24   Typ
28   Typ
38   Typ
0.035
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
Melting Point - Liquidus°F1990
Melting Point - Solidus°F1980
Densitylb/cu in. at 68°F0.322
Specific Gravity8.91
Electrical Conductivity% IACS at 68°F65
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F150
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)9.8
Specific Heat CapacityBtu/ lb /°F at 68°F0.092
Modulus of Elasticity in Tensionksi17500
Modulus of Rigidityksi6600
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingGood
Gas Shielded Arc WeldingExcellent
Coated Metal Arc WeldingNot Recommended
Spot WeldNot Recommended
Seam WeldNot Recommended
Butt WeldGood
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedExcellent
Forgeability Rating65
Machinability Rating20
Common Fabrication Processes
  • Blanking
  • Coining
  • Coppersmithing
  • Drawing
  • Etching
  • Forming and Bending
  • Heading and Upsetting
  • Hot Forging and Pressing
  • Piercing and Punching
  • Roll Threading and Knurling
  • Shearing
  • Spinning
  • Squeezing and Swaging
  • Stamping
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing7001200
Hot Treatment14001600
Typical uses
Product Category Product Reason Category Reason
AutomotiveElectrical Connectors - AutomotiveBrazing CharacteristicsBrazability
Electrical Connectors - AutomotiveConductivity (Electrical)Electrical Conductivity
Electrical Connectors - AutomotiveConductivity (Thermal)Thermal Conductivity
Electrical Connectors - AutomotiveCorrosion ResistanceCorrosion Resistance
Electrical Connectors - AutomotiveFinishing CharacteristicsEase of Tin Coating
Electrical Connectors - AutomotiveForming CharacteristicsFormability
Electrical Connectors - AutomotiveMechanical PropertiesModerate Strength
Electrical Connectors - AutomotiveSolderabilitySolderability
Fuel InjectorsCorrosion ResistanceCorrosion Resistance
Fuel InjectorsForming CharacteristicsFormability
Fuel InjectorsMechanical PropertiesFatigue Strength
Fuel InjectorsMechanical PropertiesHigh Strength
ConsumerGift Hollow WareAppearanceAppearance
Gift Hollow WareCorrosion ResistanceCorrosion Resistance
Gift Hollow WareForming CharacteristicsFormability
Gift Hollow WareMechanical PropertiesModerate Strength
ElectricalCable WrapConductivity (Electrical)Electrical Conductivity
Cable WrapConductivity (Thermal)Thermal Conductivity
Cable WrapCorrosion ResistanceCorrosion Resistance
Cable WrapCorrosion ResistanceStress Corrosion Cracking Resistance
Cable WrapDurabilityRodent Deterrence
Cable WrapForming CharacteristicsFormability
Cable WrapMechanical PropertiesFatigue Strength
Cable WrapMechanical PropertiesHigh Strength
Circuit Breaker ComponentsConductivity (Electrical)Electrical Conductivity
Circuit Breaker ComponentsConductivity (Thermal)Thermal Conductivity
Circuit Breaker ComponentsCorrosion ResistanceCorrosion Resistance
Circuit Breaker ComponentsMechanical PropertiesModerate Strength
Circuit Breaker ComponentsSoftening ResistanceResistance to Thermal Softening
Circuit Breaker ComponentsSolderabilitySolderability
ClampsConductivity (Electrical)Electrical Conductivity
ClampsConductivity (Thermal)Thermal Conductivity
ClampsCorrosion ResistanceCorrosion Resistance
ClampsMechanical PropertiesModerate Strength
Contact springsConductivity (Electrical)Electrical Conductivity
Contact springsConductivity (Thermal)Thermal Conductivity
Contact springsCorrosion ResistanceCorrosion Resistance
Contact springsMechanical PropertiesModerate Strength
Contact springsSoftening ResistanceResistance to Thermal Softening
Electrical ConnectorsConductivity (Electrical)Electrical Conductivity
Electrical ConnectorsConductivity (Thermal)Thermal Conductivity
Electrical ConnectorsCorrosion ResistanceCorrosion Resistance
Electrical ConnectorsFinishing CharacteristicsEase of Tin Coating
Electrical ConnectorsForming CharacteristicsFormability
Electrical ConnectorsMechanical PropertiesHigh Strength
Electrical SpringsConductivity (Electrical)Electrical Conductivity
Electrical SpringsConductivity (Thermal)Thermal Conductivity
Electrical SpringsCorrosion ResistanceCorrosion Resistance
Electrical SpringsForming CharacteristicsFormability
Electrical SpringsMechanical PropertiesModerate Strength
Fuse ClipsConductivity (Electrical)Electrical Conductivity
Fuse ClipsConductivity (Thermal)Thermal Conductivity
Fuse ClipsCorrosion ResistanceCorrosion Resistance
Fuse ClipsForming CharacteristicsFormability
Fuse ClipsMechanical PropertiesModerate Strength
Lead FramesConductivity (Electrical)Electrical Conductivity
Lead FramesConductivity (Thermal)Thermal Conductivity
Lead FramesCorrosion ResistanceCorrosion Resistance
Lead FramesForming CharacteristicsFormability
Lead FramesPlating CharacteristicsPlateable
Lead FramesSoftening ResistanceResistance to Softening
Plug ContactsConductivity (Electrical)Electrical Conductivity
Plug ContactsConductivity (Thermal)Thermal Conductivity
Plug ContactsCorrosion ResistanceCorrosion Resistance
Plug ContactsForming CharacteristicsFormability
Plug ContactsMechanical PropertiesModerate Strength
TerminalsConductivity (Electrical)Electrical Conductivity
TerminalsConductivity (Thermal)Thermal Conductivity
TerminalsCorrosion ResistanceCorrosion Resistance
TerminalsMechanical PropertiesModerate Strength
FastenersRivetsCorrosion ResistanceCorrosion Resistance
RivetsForming CharacteristicsFormability
RivetsMechanical PropertiesModerate Strength
IndustrialEyeletsCorrosion ResistanceCorrosion Resistance
EyeletsForming CharacteristicsFormability
EyeletsMechanical PropertiesModerate Strength
Flexible Metal HoseConductivity (Thermal)Thermal Conductivity
Flexible Metal HoseCorrosion ResistanceCorrosion Resistance
Flexible Metal HoseForming CharacteristicsFormability
Flexible Metal HoseMechanical PropertiesHigh Strength
GasketsCorrosion ResistanceCorrosion Resistance
GasketsForming CharacteristicsFormability
GasketsMechanical PropertiesModerate Strength
Welded Condenser TubesCorrosion ResistanceCorrosion Resistance
Welded Condenser TubesCorrosion ResistanceStress Corrosion Cracking Resistance
Welded Condenser TubesForming CharacteristicsFormability
Welded Condenser TubesMechanical PropertiesModerate Strength
Welded Condenser TubesSoftening ResistanceResistance to Thermal Softening
Welded Condenser TubesWelding CharacteristicsWeldability
Applicable Specifications
Form Sub-Form Specific Sub-Form System Standard Description
BarASTMB465COPPER-IRON ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
Condenser & Heat Exchanger Tube with Integral FinsWeldedASTMB956/B956MWELDED COPPER AND COPPER-ALLOY CONDENSER AND HEAT EXCHANGER TUBES WITH INTEGRAL FINS
PlateASTMB465COPPER-IRON ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
SheetASTMB465COPPER-IRON ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
ASTMB694COPPER, COPPER ALLOY AND COPPER-CLAD STAINLESS STEEL SHEET AND STRIP FOR ELECTRICAL CABLE SHIELDING
StripASTMB465COPPER-IRON ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
ASTMB694COPPER, COPPER ALLOY AND COPPER-CLAD STAINLESS STEEL SHEET AND STRIP FOR ELECTRICAL CABLE SHIELDING
Electric Connector & Spring ContactASTMB888/B88MCOPPER ALLOY STRIP FOR USE IN MANUFACTURE OF ELECTRICAL CONNECTORS OR SPRING CONTACTS
Tube, Welded Heater ExchangerWeldedASMESB543WELDED COPPER AND COPPER ALLOY TUBE
WeldedASTMB543/B543MWELDED COPPER AND COPPER ALLOY HEAT EXCHANGER TUBE
Welded Heat Exchanger & Condenser Tubewith Integral FinsASMESB956Tube, Welded, Condenser, Heat Exchanger, w/ Integral Fins
Corrosion Properties

No information available.