Find suppliers for this alloy
C19950
Elements | ||
---|---|---|
Cu(1) | Ti | |
(1) Cu + Sum of Named Elements 99.5% min. |
||
Min (%) | 3.5 | |
Max (%) | Rem | 4.5 |
Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Vickers Hardness, 3000 gm |
---|---|---|---|---|---|---|
* Measured at room temperature, 68°F (20°C). | ||||||
Strip | Super Spring | H14 |
203 Min 218 Typ 232 Max |
202 Min 217 Typ 231 Max |
0.5 Typ |
475 Typ |
Densitylb/cu in. at 68°F | 0.31 |
---|---|
Specific Gravity | 5.6 |
Electrical Conductivity% IACS at 68°F | 8 |
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 22 |
Modulus of Elasticity in Tensionksi | 19400 |
Fabrication Properties
Common Fabrication Processes
Thermal Properties
Product Category | Product | Reason Category | Reason |
---|---|---|---|
Consumer | Camera Parts | ||
Electrical | Conductors, Electrical | ||
Springs |
Applicable Specifications
Corrosion Properties