Find suppliers for this alloyC24000
Chemical Composition
Element
Cu(1)PbZnFe
(1) Cu + Sum of Named Elements 99.8% min.
Min (%)78.5
Max (%)81.50.05Rem0.05
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell F scale
Rockwell 30T scale
Shear Strength
(ksi)
Torsion Modulus
(ksi)
Fatigue Strength**
(ksi)
Ultimate Tensile Strength in Shear
(ksi)
Section Size
(in)
Flat Products1/2 HardH0261   Typ
50   Typ
18   Typ
70   Typ
64   Typ
39   Typ
0.04
1/4 HardH0153   Typ
40   Typ
30   Typ
55   Typ
54   Typ
36   Typ
0.04
HardH0474   Typ
59   Typ
7   Typ
82   Typ
71   Typ
43   Typ
5.8   Typ
0.04
Nominal Grain Size 0.015 mmOS01550   Typ
20   Typ
46   Typ
75   Typ
42   Typ
33   Typ
0.04
Nominal Grain Size 0.025 mmOS02548   Typ
17   Typ
47   Typ
69   Typ
32   Typ
0.04
Nominal Grain Size 0.035 mmOS03546   Typ
15   Typ
48   Typ
66   Typ
28   Typ
0.04
Nominal Grain Size 0.050 mmOS05044   Typ
14   Typ
50   Typ
61   Typ
16   Typ
32   Typ
0.04
Nominal Grain Size 0.070 mmOS07042   Typ
12   Typ
52   Typ
57   Typ
8   Typ
0.04
SpringH0891   Typ
65   Typ
3   Typ
91   Typ
77   Typ
48   Typ
24   Typ
0.04
Flat Products & WireHardH04107   Typ
5   Typ
53   Typ
0.08
H0474   Typ
59   Typ
7   Typ
43   Typ
0.04
Nominal Grain Size 0.015 mmOS01550   Typ
47   Typ
33   Typ
0.08
OS01550   Typ
20   Typ
46   Typ
33   Typ
0.04
Nominal Grain Size 0.050 mmOS05044   Typ
55   Typ
32   Typ
0.08
OS05044   Typ
14   Typ
50   Typ
32   Typ
0.04
SpringH0891   Typ
65   Typ
3   Typ
48   Typ
0.04
H08125   Typ
3   Typ
60   Typ
0.08
Wire1/2 HardH0282   Typ
8   Typ
47   Typ
0.08
1/4 HardH0168   Typ
12   Typ
42   Typ
0.08
1/8 HardH0056   Typ
27   Typ
37   Typ
0.08
Extra HardH06116   Typ
4   Typ
0.08
HardH04107   Typ
5   Typ
53   Typ
23   Typ
0.08
Nominal Grain Size 0.015 mmOS01550   Typ
47   Typ
33   Typ
0.08
Nominal Grain Size 0.035 mmOS03546   Typ
50   Typ
0.08
Nominal Grain Size 0.050 mmOS05044   Typ
55   Typ
32   Typ
0.08
SpringH08125   Typ
3   Typ
60   Typ
26   Typ
0.08
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
Melting Point - Liquidus°F1830
Melting Point - Solidus°F1770
Densitylb/cu in. at 68°F0.313
Specific Gravity8.67
Electrical Conductivity% IACS at 68°F32
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F81
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)10.6
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi16000
Modulus of Rigidityksi6000
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingGood
Gas Shielded Arc WeldingGood
Coated Metal Arc WeldingNot Recommended
Spot WeldFair
Seam WeldNot Recommended
Butt WeldGood
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedFair
Machinability Rating30
Common Fabrication Processes
  • Blanking
  • Drawing
  • Etching
  • Forming and Bending
  • Heading and Upsetting
  • Piercing and Punching
  • Roll Threading and Knurling
  • Shearing
  • Spinning
  • Squeezing and Swaging
  • Stamping
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing8001300
Hot Treatment15001650
Typical uses
Product Category Product Reason Category Reason
ArchitectureMedallionsAppearanceAppearance
MedallionsCorrosion ResistanceCorrosion Resistance
Ornamental ComponentsAppearanceAppearance
Ornamental ComponentsCorrosion ResistanceCorrosion Resistance
Ornamental ComponentsMechanical PropertiesModerate Strength
SpandrelsCorrosion ResistanceCorrosion Resistance
SpandrelsForming CharacteristicsFormability
SpandrelsMechanical PropertiesModerate Strength
Builders HardwareDecorative PanelsAppearanceAppearance
Decorative PanelsCorrosion ResistanceCorrosion Resistance
Decorative PanelsMechanical PropertiesModerate Strength
ConsumerClock DialsAppearanceAppearance
Musical Instrument PartsAppearanceAppearance
Musical Instrument PartsCorrosion ResistanceCorrosion Resistance
Musical Instrument PartsForming CharacteristicsFormability
PlaquesAppearanceAppearance
PlaquesCorrosion ResistanceCorrosion Resistance
ElectricalBattery CapsConductivity (Electrical)Electrical Conductivity
Battery CapsCorrosion ResistanceCorrosion Resistance
Battery CapsForming CharacteristicsFormability
Battery CapsMechanical PropertiesModerate Strength
Rotor Bars, AC MotorsBrazing CharacteristicsBrazability
Rotor Bars, AC MotorsConductivity (Electrical)Electrical Resistivity
IndustrialFlexible HoseCorrosion ResistanceCorrosion Resistance
Flexible HoseMechanical PropertiesModerate Strength
Flexible HoseSolderabilitySolderability
Flexible Hose BellowsCorrosion ResistanceCorrosion Resistance
Flexible Hose BellowsCorrosion ResistanceStress Corrosion Cracking Resistance
Flexible Hose BellowsMechanical PropertiesDuctility
Flexible Hose BellowsMechanical PropertiesModerate to High Strength
Pump LinesCorrosion ResistanceCorrosion Resistance
Pump LinesForming CharacteristicsFormability
Pump LinesMechanical PropertiesModerate Strength
Pump LinesSolderabilitySolderability
Welding WireOtherBlended with C18400 to produce C22000
OtherTokensAppearanceAppearance
TokensCorrosion ResistanceCorrosion Resistance
TokensForming CharacteristicsFormability
TokensMechanical PropertiesModerate Strength
Applicable Specifications
Form System Standard Description
BarASTMB19CARTRIDGE BRASS SHEET, STRIP, PLATE, BAR AND DISKS
ASTMB36/B36MBRASS PLATE, SHEET, STRIP AND ROLLED BAR
Brazing Filler MetalFEDERALQQ-B-650BRAZING ALLOY, COPPER, COPPER-ZINC, AND COPPER-PHOSPHORUS
CupsASTMB19CARTRIDGE BRASS SHEET, STRIP, PLATE, BAR AND DISKS
PlateASTMB19CARTRIDGE BRASS SHEET, STRIP, PLATE, BAR AND DISKS
ASTMB36/B36MBRASS PLATE, SHEET, STRIP AND ROLLED BAR
Rod, Bar & ShapesASTMB927/B927MBRASS ROD, BAR, AND SHAPES
SheetASTMB36/B36MBRASS PLATE, SHEET, STRIP AND ROLLED BAR
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
StripASTMB36/B36MBRASS PLATE, SHEET, STRIP AND ROLLED BAR
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
Strip, Sheet & PlateASTMB19CARTRIDGE BRASS SHEET, STRIP, PLATE, BAR AND DISKS
WireASTMB134/B134MBRASS WIRE
Corrosion Properties