Find suppliers for this alloyC25600
Element | ||||
---|---|---|---|---|
Cu(1) | Pb | Zn | Fe | |
(1) Cu + Sum of Named Elements 99.7% min. | ||||
Min (%) | 71.0 | |||
Max (%) | 73.0 | 0.05 | Rem | 0.05 |
Mechanical Properties
Melting Point - Liquidus°F | 1765 |
---|---|
Melting Point - Solidus°F | 1697 |
Densitylb/cu in. at 68°F | 0.309 |
Specific Gravity | 8.56 |
Electrical Conductivity% IACS at 68°F | 36.5 |
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 72 |
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F) | 10.9 |
Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
Modulus of Elasticity in Tensionksi | 16000 |
Modulus of Rigidityksi | 6000 |
Fabrication Properties
Fabrication Process Properties
Thermal Characteristics
Typical Uses
Applicable Specifications
Corrosion Properties