Find suppliers for this alloy
C26000
| Elements | ||||
|---|---|---|---|---|
| Cu(1) | Pb | Zn | Fe | |
|
(1) Cu + Sum of Named Elements 99.7% min. |
||||
| Min (%) | 68.5 | |||
| Max (%) | 71.5 | 0.07 | Rem | 0.05 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Rockwell F scale | Rockwell 30T scale | Shear Strength (ksi) |
Torsion Modulus (ksi) |
Fatigue Strength** (ksi) |
Section Size (in) |
Cold Work (%) |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | |||||||||||||
| Flat Products | 1/2 Hard | H02 |
62 Typ |
25 Typ |
70 Typ |
65 Typ |
40 Typ |
18 Typ | 0.04 | ||||
| 1/4 Hard | H01 |
54 Typ |
40 Typ |
43 Typ |
55 Typ |
54 Typ |
36 Typ |
0.04 | |||||
| Extra Hard | H06 |
86 Typ |
65 Typ |
5 Typ |
88 Typ |
76 Typ |
46 Typ |
0.04 | |||||
| Extra Spring | H10 |
99 Typ |
65 Typ |
3 Typ |
93 Typ |
78 Typ |
0.04 | ||||||
| Hard | H04 |
76 Typ |
63 Typ |
8 Typ |
82 Typ |
73 Typ |
44 Typ |
21 Typ | 0.04 | ||||
| Nominal Grain Size 0.015 mm | OS015 |
53 Typ |
22 Typ |
54 Typ |
78 Typ |
43 Typ |
35 Typ |
14 Typ | 0.04 | ||||
| Nominal Grain Size 0.025 mm | OS025 |
51 Typ |
19 Typ |
55 Typ |
72 Typ |
36 Typ |
0.04 | ||||||
| Nominal Grain Size 0.035 mm | OS035 |
49 Typ |
17 Typ |
57 Typ |
68 Typ |
31 Typ |
34 Typ |
14 Typ | 0.04 | ||||
| Nominal Grain Size 0.050 mm | OS050 |
47 Typ |
15 Typ |
62 Typ |
64 Typ |
26 Typ |
0.04 | ||||||
| Nominal Grain Size 0.070 mm | OS070 |
46 Typ |
14 Typ |
65 Typ |
58 Typ |
15 Typ |
32 Typ |
13 Typ | 0.04 | ||||
| Nominal Grain Size 0.100 mm | OS100 |
44 Typ |
11 Typ |
66 Typ |
54 Typ |
11 Typ |
13 Typ | 0.04 | |||||
| Spring | H08 |
94 Typ |
65 Typ |
3 Typ |
91 Typ |
77 Typ |
48 Typ |
23 Typ | 0.04 | ||||
| Rod | 1/2 Hard | H02 |
70 Typ |
30 Typ |
80 Typ |
42 Typ |
22 Typ | 1 | 20 | ||||
| 1/8 Hard | H00 |
55 Typ |
40 Typ |
48 Typ |
60 Typ |
36 Typ |
5.8 Typ | 1 | 6 | ||||
| Nominal Grain Size 0.050 mm | OS050 |
48 Typ |
16 Typ |
65 Typ |
65 Typ |
34 Typ |
1 | ||||||
| Tube | Hard Drawn | H80 |
78 Typ |
8 Typ |
82 Typ |
73 Typ |
35 | ||||||
| Nominal Grain Size 0.025 mm | OS025 |
52 Typ |
20 Typ |
55 Typ |
75 Typ |
40 Typ |
|||||||
| Nominal Grain Size 0.050 mm | OS050 |
47 Typ |
15 Typ |
65 Typ |
64 Typ |
26 Typ |
|||||||
| Wire | 1/4 Hard | H01 |
70 Typ |
20 Typ |
0.08 | ||||||||
| 1/8 Hard | H00 |
58 Typ |
35 Typ |
38 Typ |
0.08 | ||||||||
| Extra Hard | H06 |
124 Typ |
4 Typ |
0.08 | |||||||||
| Nominal Grain Size 0.015 mm | OS015 |
54 Typ |
56 Typ |
0.08 | |||||||||
| Nominal Grain Size 0.025 mm | OS025 |
52 Typ |
58 Typ |
0.08 | |||||||||
| Nominal Grain Size 0.035 mm | OS035 |
50 Typ |
60 Typ |
34 Typ |
0.08 | ||||||||
| Nominal Grain Size 0.050 mm | OS050 |
48 Typ |
64 Typ |
0.08 | |||||||||
| Spring | H08 |
130 Typ |
3 Typ |
60 Typ |
22 Typ | 0.08 | |||||||
| Melting Point - Liquidus°F | 1750 |
|---|---|
| Melting Point - Solidus°F | 1680 |
| Densitylb/cu in. at 68°F | 0.308 |
| Specific Gravity | 8.53 |
| Electrical Conductivity% IACS at 68°F | 28 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 70 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 11.1 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 16000 |
| Modulus of Rigidityksi | 6000 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Good |
| Gas Shielded Arc Welding | Good |
| Coated Metal Arc Welding | Not Recommended |
| Spot Weld | Fair |
| Seam Weld | Not Recommended |
| Butt Weld | Good |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Fair |
| Machinability Rating | 30 |
Common Fabrication Processes
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 800 | 1400 | ||
| Hot Working Temperature | 1350 | 1550 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Architecture | Grillwork | Corrosion Resistance | Corrosion Resistance |
| Grillwork | Forming Characteristics | Formability | |
| Grillwork | Mechanical Properties | Moderate Strength | |
| Automotive | Electrical Connectors | Conductivity (Electrical) | Electrical Conductivity |
| Electrical Connectors | Corrosion Resistance | Corrosion Resistance | |
| Electrical Connectors | Forming Characteristics | Formability | |
| Heater Cores | Corrosion Resistance | Corrosion Resistance | |
| Heater Cores | Forming Characteristics | Formability | |
| Heater Cores | Mechanical Properties | Moderate Strength | |
| Odometer Contacts | Conductivity (Electrical) | Electrical Conductivity | |
| Odometer Contacts | Forming Characteristics | Formability | |
| Odometer Contacts | Friction & Wear Properties | Wear Resistance | |
| Radiator Cores | Corrosion Resistance | Corrosion Resistance | |
| Radiator Cores | Mechanical Properties | Moderate Strength | |
| Radiator Tanks | Brazing Characteristics | Brazability | |
| Radiator Tanks | Conductivity (Thermal) | Thermal Conductivity | |
| Radiator Tanks | Corrosion Resistance | Corrosion Resistance | |
| Radiator Tanks | Forming Characteristics | Formability | |
| Radiator Tanks | Mechanical Properties | Moderate Strenght | |
| Radiator Tanks | Solderability | Solderability | |
| Radiator Tube | Brazing Characteristics | Brazability | |
| Radiator Tube | Conductivity (Thermal) | Thermal Conductivity | |
| Radiator Tube | Corrosion Resistance | Corrosion Resistance | |
| Radiator Tube | Forming Characteristics | Formability | |
| Radiator Tube | Mechanical Properties | Moderate Strength | |
| Radiator Tube | Solderability | Solderability | |
| Tanks | Corrosion Resistance | Corrosion Resistance | |
| Tanks | Forming Characteristics | Formability | |
| Tanks | Mechanical Properties | Moderate Strength | |
| Thermostats | Corrosion Resistance | Corrosion Resistance | |
| Thermostats | Forming Characteristics | Formability | |
| Thermostats | Mechanical Properties | Moderate Strength | |
| Builders Hardware | Decorative Hardware | Appearance | Appearance |
| Decorative Hardware | Corrosion Resistance | Corrosion Resistance | |
| Decorative Hardware | Mechanical Properties | Moderate Strength | |
| Door Knobs | Appearance | Appearance | |
| Door Knobs | Corrosion Resistance | Corrosion Resistance | |
| Door Knobs | Forming Characteristics | Formability | |
| Finish Hardware | Appearance | Appearance | |
| Finish Hardware | Corrosion Resistance | Corrosion Resistance | |
| Finish Hardware | Mechanical Properties | Moderate Strength | |
| Hinges | Appearance | Appearance | |
| Hinges | Corrosion Resistance | Corrosion Resistance | |
| Hinges | Mechanical Properties | Moderate Strength | |
| Kick Plates | Appearance | Appearance | |
| Kick Plates | Corrosion Resistance | Corrosion Resistance | |
| Locks | Appearance | Appearance | |
| Locks | Corrosion Resistance | Corrosion Resistance | |
| Locks | Mechanical Properties | Moderate Strength | |
| Push Plates | Appearance | Appearance | |
| Push Plates | Corrosion Resistance | Corrosion Resistance | |
| Push Plates | Mechanical Properties | Moderate Strength | |
| Consumer | Bird Cages | Appearance | Appearance |
| Bird Cages | Corrosion Resistance | Corrosion Resistance | |
| Bird Cages | Forming Characteristics | Formability | |
| Bird Cages | Mechanical Properties | Moderate Strength | |
| Buttons | Appearance | Appearance | |
| Buttons | Corrosion Resistance | Corrosion Resistance | |
| Buttons | Forming Characteristics | Formability | |
| Buttons | Mechanical Properties | Moderate Strength | |
| Buttons | Mechanical Properties | Retention of Spring Properties | |
| Buttons | Plating Characteristics | Plateable | |
| Chain Links | Corrosion Resistance | Corrosion Resistance | |
| Chain Links | Forming Characteristics | Blanking Characteristics | |
| Coinage | Appearance | Appearance | |
| Coinage | Corrosion Resistance | Corrosion Resistance | |
| Coinage | Forming Characteristics | Coinability | |
| Coinage | Forming Characteristics | Formability | |
| Coinage | Plating Characteristics | Plateable | |
| Costume Jewelry | Appearance | Appearance | |
| Costume Jewelry | Corrosion Resistance | Corrosion Resistance | |
| Costume Jewelry | Forming Characteristics | Formability | |
| Costume Jewelry | Mechanical Properties | Retention of Spring Properties | |
| Costume Jewelry | Plating Characteristics | Plateable | |
| Etched Articles | Appearance | Appearance | |
| Etched Articles | Corrosion Resistance | Corrosion Resistance | |
| Etched Articles | Forming Characteristics | Formability | |
| Etched Articles | Mechanical Properties | Moderate Strength | |
| Fireplace Screens | Appearance | Appearance | |
| Fireplace Screens | Corrosion Resistance | Corrosion Resistance | |
| Fireplace Screens | Mechanical Properties | Moderate Strength | |
| Lamps | Appearance | Appearance | |
| Lamps | Corrosion Resistance | Corrosion Resistance | |
| Lamps | Mechanical Properties | Moderate Strength | |
| Pen/Pencil Inserts and Clips | Forming Characteristics | Formability | |
| Pen/Pencil Inserts and Clips | Mechanical Properties | Moderate Strength | |
| Planters | Appearance | Appearance | |
| Planters | Corrosion Resistance | Corrosion Resistance | |
| Shells - Electrical Sockets | Conductivity (Electrical) | Electrical Conductivity | |
| Shells - Electrical Sockets | Conductivity (Thermal) | Thermal Conductivity | |
| Shells - Electrical Sockets | Corrosion Resistance | Corrosion Resistance | |
| Shells - Electrical Sockets | Drawing Characteristics | Drawability | |
| Shells - Electrical Sockets | Machining Characteristics | Low Tool and Maintenance Costs | |
| Shells - Electrical Sockets | Mechanical Properties | Moderate Strength | |
| Snaps | Appearance | Appearance | |
| Snaps | Corrosion Resistance | Corrosion Resistance | |
| Snaps | Forming Characteristics | Formability | |
| Snaps | Mechanical Properties | Moderate Strength | |
| Snaps | Mechanical Properties | Retention of Spring Properties | |
| Snaps | Plating Characteristics | Plateable | |
| Syringe Parts | Corrosion Resistance | Corrosion Resistance | |
| Syringe Parts | Corrosion Resistance | Corrosion Resistance to Chemicals | |
| Syringe Parts | Forming Characteristics | Formability | |
| Syringe Parts | Mechanical Properties | Moderate Strength | |
| Watch Parts | Corrosion Resistance | Corrosion Resistance | |
| Watch Parts | Forming Characteristics | Formability | |
| Watch Parts | Friction & Wear Properties | Wear Resistance | |
| Electrical | Flashlight Shells | Corrosion Resistance | Corrosion Resistance |
| Flashlight Shells | Forming Characteristics | Formability | |
| Flashlight Shells | Mechanical Properties | Moderate Strength | |
| Lamp Fixtures | Appearance | Appearance | |
| Lamp Fixtures | Corrosion Resistance | Corrosion Resistance | |
| Lamp Fixtures | Mechanical Properties | Moderate Strength | |
| Reflectors | Appearance | Appearance | |
| Reflectors | Corrosion Resistance | Corrosion Resistance | |
| Reflectors | Mechanical Properties | Moderate Strength | |
| Screw Shells | Corrosion Resistance | Corrosion Resistance | |
| Screw Shells | Forming Characteristics | Formability | |
| Screw Shells | Mechanical Properties | Moderate Strength | |
| Terminal Connectors | Conductivity (Electrical) | Electrical Conductivity | |
| Terminal Connectors | Conductivity (Thermal) | Thermal Conductivity | |
| Terminal Connectors | Corrosion Resistance | Corrosion Resistance | |
| Terminal Connectors | Forming Characteristics | Formability | |
| Terminal Connectors | Mechanical Properties | Moderate Strength | |
| Fasteners | Eyelets | Appearance | Appearance |
| Eyelets | Corrosion Resistance | Corrosion Resistance | |
| Eyelets | Forming Characteristics | Formability | |
| Eyelets | Mechanical Properties | Moderate Strength | |
| Fasteners | Corrosion Resistance | Corrosion Resistance | |
| Fasteners | Forming Characteristics | Formability | |
| Fasteners | Mechanical Properties | Moderate Strength | |
| Grommets | Appearance | Appearance | |
| Grommets | Corrosion Resistance | Corrosion Resistance | |
| Grommets | Forming Characteristics | Formability | |
| Grommets | Mechanical Properties | Moderate Strength | |
| Pins | Appearance | Appearance | |
| Pins | Corrosion Resistance | Corrosion Resistance | |
| Pins | Mechanical Properties | Moderate Strength | |
| Rivets | Appearance | Appearance | |
| Rivets | Corrosion Resistance | Corrosion Resistance | |
| Rivets | Forming Characteristics | Formability | |
| Rivets | Mechanical Properties | Moderate Strength | |
| Screws | Appearance | Appearance | |
| Screws | Corrosion Resistance | Corrosion Resistance | |
| Screws | Forming Characteristics | Formability | |
| Screws | Mechanical Properties | Moderate Strength | |
| Industrial | Air Pressure Conveyer Systems | Corrosion Resistance | Corrosion Resistance |
| Air Pressure Conveyer Systems | Forming Characteristics | Formability | |
| Air Pressure Conveyer Systems | Mechanical Properties | Moderate Strength | |
| Bead Chain | Corrosion Resistance | Corrosion Resistance | |
| Bead Chain | Forming Characteristics | Formability | |
| Bead Chain | Mechanical Properties | Moderate Strength | |
| Chain | Corrosion Resistance | Corrosion Resistance | |
| Chain | Forming Characteristics | Formability | |
| Chain | Mechanical Properties | Moderate Strength | |
| Heat Exchangers | Brazing Characteristics | Brazability | |
| Heat Exchangers | Conductivity (Thermal) | Thermal Conductivity | |
| Heat Exchangers | Corrosion Resistance | Corrosion Resistance | |
| Heat Exchangers | Forming Characteristics | Formability | |
| Heat Exchangers | Mechanical Properties | Moderate Strength | |
| Heat Exchangers | Solderability | Solderability | |
| Liners | Corrosion Resistance | Corrosion Resistance | |
| Liners | Forming Characteristics | Formability | |
| Liners | Mechanical Properties | Moderate Strength | |
| Power Cylinders | Corrosion Resistance | Corrosion Resistance | |
| Power Cylinders | Forming Characteristics | Formability | |
| Power Cylinders | Mechanical Properties | Moderate Strength | |
| Pump Cylinders | Corrosion Resistance | Corrosion Resistance | |
| Pump Cylinders | Forming Characteristics | Formability | |
| Pump Cylinders | Mechanical Properties | Moderate Strength | |
| Pumps | Corrosion Resistance | Corrosion Resistance | |
| Pumps | Forming Characteristics | Formability | |
| Pumps | Mechanical Properties | Moderate Strength | |
| Sound Proofing Equipment | Damping Characteristics | Damping Characteristics | |
| Springs | Corrosion Resistance | Corrosion Resistance | |
| Springs | Forming Characteristics | Formability | |
| Springs | Mechanical Properties | High Modulus of Elasticity | |
| Springs | Mechanical Properties | Moderate Strength | |
| Tubing for Instruments and Machines | Corrosion Resistance | Corrosion Resistance | |
| Tubing for Instruments and Machines | Forming Characteristics | Formability | |
| Tubing for Instruments and Machines | Mechanical Properties | Moderate Strength | |
| Tubing for Instruments and Machines | Welding Characteristics | Weldability | |
| Wire Screens | Appearance | Appearance | |
| Wire Screens | Corrosion Resistance | Corrosion Resistance | |
| Wire Screens | Mechanical Properties | Moderate Strength | |
| Ordnance | Ammunition | Forming Characteristics | Formability |
| Ammunition Cartridge Cases | Corrosion Resistance | Corrosion Resistance | |
| Ammunition Cartridge Cases | Drawing Characteristics | Deep Drawing Capability | |
| Ammunition Cartridge Cases | Mechanical Properties | Moderate Strength | |
| Mechanical Housings for Lighters | Corrosion Resistance | Corrosion Resistance | |
| Mechanical Housings for Lighters | Drawing Characteristics | Drawability | |
| Mechanical Housings for Lighters | Machining Characteristics | Low Tool and Maintenance Costs | |
| Mechanical Housings for Lighters | Mechanical Properties | Moderate Strength | |
| Mechanical Housings for Lighters | Plating Characteristics | Plateable | |
| Shells - Mechanical Housings for Ammunition | Corrosion Resistance | Corrosion Resistance | |
| Shells - Mechanical Housings for Ammunition | Drawing Characteristics | Drawability | |
| Shells - Mechanical Housings for Ammunition | Machining Characteristics | Low Tool and Maintenance Costs | |
| Shells - Mechanical Housings for Ammunition | Mechanical Properties | Moderate Strength | |
| Shells - Mechanical Housings for Ammunition | Plating Characteristics | Plateable | |
| Other | Stencils | Appearance | Appearance |
| Stencils | Corrosion Resistance | Corrosion Resistance | |
| Stencils | Forming Characteristics | Blanking Characteristics | |
| Washers | Corrosion Resistance | Corrosion Resistance | |
| Washers | Forming Characteristics | Blanking Characteristics | |
| Plumbing | Bathroom Fixtures | Corrosion Resistance | Corrosion Resistance |
| Bathroom Fixtures | Forming Characteristics | Formability | |
| Bathroom Fixtures | Mechanical Properties | Moderate Strength | |
| Faucet Escutcheons | Corrosion Resistance | Corrosion Resistance | |
| Faucet Escutcheons | Forming Characteristics | Formability | |
| Faucet Escutcheons | Mechanical Properties | Moderate Strength | |
| Faucet Escutcheons | Plating Characteristics | Plateable | |
| Fittings | Corrosion Resistance | Corrosion Resistance | |
| Fittings | Forming Characteristics | Formability | |
| Fittings | Mechanical Properties | Moderate Strength | |
| Plumbing Accessories | Corrosion Resistance | Corrosion Resistance | |
| Plumbing Accessories | Forming Characteristics | Formability | |
| Plumbing Accessories | Mechanical Properties | Moderate Strength | |
| Plumbing Accessories | Plating Characteristics | Plateable | |
| Plumbing Brass Goods | Appearance | Appearance | |
| Plumbing Brass Goods | Corrosion Resistance | Corrosion Resistance | |
| Plumbing Brass Goods | Forming Characteristics | Formability | |
| Plumbing Brass Goods | Mechanical Properties | Moderate Strength | |
| Traps | Appearance | Appearance | |
| Traps | Corrosion Resistance | Corrosion Resistance | |
| Traps | Mechanical Properties | Moderate Strength |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Bar | ASTM | B36/B36M | BRASS PLATE, SHEET, STRIP AND ROLLED BAR | ||
| SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | |||
| ASTM | B19 | CARTRIDGE BRASS SHEET, STRIP, PLATE, BAR AND DISKS | |||
| SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |||
| Brazing Filler Metal | FEDERAL | QQ-B-650 | BRAZING ALLOY, COPPER, COPPER-ZINC, AND COPPER-PHOSPHORUS | ||
| Cartridge Brass Cups | ASTM | B129 | CARTRIDGE BRASS CARTRIDGE CASE CUPS | ||
| Cups | MILITARY | MIL-C-10375 | CUPS, CASE, CARTRIDGE, COPPER ALLOY (FOR SMALL ARMS AMMUNITION) | ||
| Disks | ASTM | B19 | CARTRIDGE BRASS SHEET, STRIP, PLATE, BAR AND DISKS | ||
| Plate | ASTM | B36/B36M | BRASS PLATE, SHEET, STRIP AND ROLLED BAR | ||
| ASTM | B19 | CARTRIDGE BRASS SHEET, STRIP, PLATE, BAR AND DISKS | |||
| AMS | 4505 | BRASS SHEET, STRIP AND PLATE, ANNEALED | |||
| AMS | 4507 | BRASS SHEET, STRIP AND PLATE, HALF-HARD | |||
| Rod | SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | ||
| SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |||
| Rod, Bar & Shapes | ASTM | B927/B927M | BRASS ROD, BAR, AND SHAPES | ||
| Sheet | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | |||
| AMS | 4507 | BRASS SHEET, STRIP AND PLATE, HALF-HARD | |||
| AMS | 4505 | BRASS SHEET, STRIP AND PLATE, ANNEALED | |||
| ASTM | B36/B36M | BRASS PLATE, SHEET, STRIP AND ROLLED BAR | |||
| AMS | 4508 | BRASS SHEET, LAMINATED SURFACE BONDED | |||
| ASTM | B19 | CARTRIDGE BRASS SHEET, STRIP, PLATE, BAR AND DISKS | |||
| Shim stock | Laminate | MILITARY | MIL-S-22499 | SHIM STOCK, LAMINATED | |
| Strip | ASTM | B19 | CARTRIDGE BRASS SHEET, STRIP, PLATE, BAR AND DISKS | ||
| SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | |||
| ASTM | B36/B36M | BRASS PLATE, SHEET, STRIP AND ROLLED BAR | |||
| AMS | 4507 | BRASS SHEET, STRIP AND PLATE, HALF-HARD | |||
| AMS | 4505 | BRASS SHEET, STRIP AND PLATE, ANNEALED | |||
| ASTM | B569 | BRASS STRIP IN NARROW WIDTHS AND LIGHT GAGE FOR HEAT EXCHANGER TUBING | |||
| ASTM | B888/B88M | COPPER ALLOY STRIP FOR USE IN MANUFACTURE OF ELECTRICAL CONNECTORS OR SPRING CONTACTS | |||
| SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |||
| Tube | SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | ||
| Seamless | ASME | SB135 | SEAMLESS BRASS TUBE | ||
| ASTM | B587 | WELDED BRASS TUBE | |||
| Seamless (Metric) | ASTM | B135/B135M | Seamless Brass Tube | ||
| MILITARY | MIL-T-20219 | TUBES, BRASS, VOICE AND PNEUMATIC | |||
| ASTM | B135 | Tube, Seamless | |||
| SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |||
| FEDERAL | WW-T-791 | TUBING: BRASS, SEAMLESS | |||
| ASTM | B587 | WELDED BRASS TUBE | |||
| Wire | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | |||
| ASTM | B134/B134M | BRASS WIRE |
Corrosion Properties