Find suppliers for this alloyC26100
Chemical Composition
Element
Cu(1)PbZnFePAs
(1) Cu + Sum of Named Elements 99.7% min.
Min (%)68.50.020.02
Max (%)71.50.05Rem0.050.050.06
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell F scale
Rockwell 30T scale
Shear Strength
(ksi)
Fatigue Strength**
(ksi)
Section Size
(in)
Cold Work
(%)
Flat Products1/2 HardH0262   Typ
52   Typ
25   Typ
70   Typ
65   Typ
40   Typ
18   Typ
0.04
1/4 HardH0154   Typ
40   Typ
43   Typ
55   Typ
54   Typ
36   Typ
0.04
Extra HardH0686   Typ
65   Typ
5   Typ
88   Typ
76   Typ
46   Typ
0.04
Extra SpringH1099   Typ
65   Typ
3   Typ
93   Typ
78   Typ
0.04
HardH0476   Typ
63   Typ
8   Typ
82   Typ
73   Typ
44   Typ
21   Typ
0.04
Nominal Grain Size 0.015 mmOS01553   Typ
22   Typ
54   Typ
78   Typ
43   Typ
35   Typ
14   Typ
0.04
Nominal Grain Size 0.025 mmOS02551   Typ
19   Typ
55   Typ
72   Typ
36   Typ
0.04
Nominal Grain Size 0.035 mmOS03549   Typ
17   Typ
57   Typ
68   Typ
31   Typ
34   Typ
14   Typ
0.04
Nominal Grain Size 0.050 mmOS05047   Typ
15   Typ
62   Typ
64   Typ
26   Typ
0.04
Nominal Grain Size 0.070 mmOS07046   Typ
14   Typ
65   Typ
58   Typ
15   Typ
32   Typ
13   Typ
0.04
Nominal Grain Size 0.100 mmOS10044   Typ
11   Typ
66   Typ
54   Typ
11   Typ
13   Typ
0.04
SpringH0894   Typ
65   Typ
3   Typ
91   Typ
77   Typ
48   Typ
23   Typ
0.04
Rod1/2 HardH0270   Typ
52   Typ
30   Typ
80   Typ
42   Typ
22   Typ
120
1/8 HardH0055   Typ
40   Typ
48   Typ
60   Typ
36   Typ
16
Nominal Grain Size 0.050 mmOS05048   Typ
16   Typ
65   Typ
65   Typ
34   Typ
1
TubeNominal Grain Size 0.025 mmOS02552   Typ
20   Typ
55   Typ
75   Typ
40   Typ
Nominal Grain Size 0.050 mmOS05047   Typ
15   Typ
65   Typ
64   Typ
26   Typ
Solution Heat Treated and Cold Worked: HardTD0478   Typ
64   Typ
8   Typ
82   Typ
73   Typ
35
Wire1/4 HardH0170   Typ
20   Typ
0.08
1/8 HardH0058   Typ
35   Typ
38   Typ
0.08
Extra HardH06124   Typ
4   Typ
0.08
Nominal Grain Size 0.015 mmOS01554   Typ
56   Typ
0.08
Nominal Grain Size 0.025 mmOS02552   Typ
58   Typ
0.08
Nominal Grain Size 0.035 mmOS03550   Typ
60   Typ
34   Typ
0.08
Nominal Grain Size 0.050 mmOS05048   Typ
64   Typ
0.08
SpringH08130   Typ
3   Typ
60   Typ
22   Typ
0.08
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
Melting Point - Liquidus°F1750
Melting Point - Solidus°F1680
Densitylb/cu in. at 68°F0.308
Specific Gravity8.53
Electrical Conductivity% IACS at 68°F28
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F70
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)11.1
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi16000
Modulus of Rigidityksi6000
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingGood
Gas Shielded Arc WeldingFair
Coated Metal Arc WeldingNot Recommended
Spot WeldGood
Seam WeldNot Recommended
Butt WeldGood
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedFair
Fabrication Process Properties

No fabrication process properties for this alloy

    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing8001400
Hot Treatment13501550
Typical uses
Product Category Product Reason Category Reason
ArchitectureGrillworkAppearanceAppearance
GrillworkCorrosion ResistanceCorrosion Resistance
GrillworkMechanical PropertiesModerate Strength
GrillworkPlating CharacteristicsPlateable
AutomotiveHeater CordCorrosion ResistanceCorrosion Resistance
Heater CordForming CharacteristicsFormability
Heater CordMechanical PropertiesModerate Strength
RadiatorsCorrosion ResistanceCorrosion Resistance
RadiatorsForming CharacteristicsFormability
RadiatorsMechanical PropertiesModerate Strength
RadiatorsSolderabilitySolderability
RadiatorsWelding CharacteristicsWeldability
TanksCorrosion ResistanceCorrosion Resistance
TanksForming CharacteristicsFormability
TanksMechanical PropertiesModerate Strength
TanksSolderabilitySolderability
TanksWelding CharacteristicsWeldability
Builders HardwareFinish HardwareAppearanceAppearance
Finish HardwareMechanical PropertiesModerate Strength
Finish HardwarePlating CharacteristicsPlateable
HingesAppearanceAppearance
HingesCorrosion ResistanceCorrosion Resistance
HingesMechanical PropertiesModerate Strength
HingesPlating CharacteristicsPlateable
Kick PlatesAppearanceAppearance
Kick PlatesCorrosion ResistanceCorrosion Resistance
Kick PlatesMechanical PropertiesModerate Strength
Kick PlatesPlating CharacteristicsPlateable
LocksAppearanceAppearance
LocksCorrosion ResistanceCorrosion Resistance
LocksMechanical PropertiesModerate Strength
Push PlatesAppearanceAppearance
Push PlatesCorrosion ResistanceCorrosion Resistance
Push PlatesMechanical PropertiesModerate Strength
StencilsCorrosion ResistanceCorrosion Resistance
StencilsMechanical PropertiesModerate Strength
StencilsPlating CharacteristicsPlateable
ElectricalFlashlight ShellsCorrosion ResistanceCorrosion Resistance
Flashlight ShellsForming CharacteristicsFormability
Flashlight ShellsMechanical PropertiesModerate Strength
Lamp FixturesAppearanceAppearance
Lamp FixturesAppearanceColor
Lamp FixturesCorrosion ResistanceCorrosion Resistance
Lamp FixturesForming CharacteristicsFormability
Lamp FixturesMechanical PropertiesModerate Strength
ReflectorsAppearanceAppearance
ReflectorsCorrosion ResistanceCorrosion Resistance
ReflectorsMechanical PropertiesModerate Strength
Screw ShellsCorrosion ResistanceCorrosion Resistance
Screw ShellsForming CharacteristicsFormability
Screw ShellsMechanical PropertiesModerate Strength
Socket ShellsCorrosion ResistanceCorrosion Resistance
Socket ShellsForming CharacteristicsFormability
Socket ShellsMechanical PropertiesModerate Strength
FastenersEyeletsAppearanceAppearance
EyeletsCorrosion ResistanceCorrosion Resistance
EyeletsMechanical PropertiesModerate Strength
EyeletsPlating CharacteristicsPlateable
FastenersAppearanceAppearance
FastenersCorrosion ResistanceCorrosion Resistance
FastenersForming CharacteristicsFormability
FastenersMechanical PropertiesModerate Strength
FastenersPlating CharacteristicsPlateable
GrommetsAppearanceAppearance
GrommetsCorrosion ResistanceCorrosion Resistance
GrommetsForming CharacteristicsFormability
GrommetsMechanical PropertiesModerate Strength
PinsAppearanceAppearance
PinsCorrosion ResistanceCorrosion Resistance
PinsMechanical PropertiesModerate Strength
RivetsAppearanceAppearance
RivetsCorrosion ResistanceCorrosion Resistance
RivetsForming CharacteristicsFormability
RivetsMechanical PropertiesModerate Strength
ScrewsCorrosion ResistanceCorrosion Resistance
ScrewsForming CharacteristicsFormability
ScrewsMechanical PropertiesModerate Strength
IndustrialBead ChainAppearanceAppearance
Bead ChainAppearanceColor
Bead ChainCorrosion ResistanceCorrosion Resistance
Bead ChainForming CharacteristicsFormability
Bead ChainMechanical PropertiesModerate Strength
ChainCorrosion ResistanceCorrosion Resistance
ChainForming CharacteristicsFormability
ChainMechanical PropertiesModerate Strength
LinersAppearanceAppearance
LinersCorrosion ResistanceCorrosion Resistance
LinersForming CharacteristicsFormability
LinersMechanical PropertiesModerate Strength
Power CylindersCorrosion ResistanceCorrosion Resistance
Power CylindersForming CharacteristicsFormability
Power CylindersFriction & Wear PropertiesWear Resistance
Power CylindersMechanical PropertiesHigh Modulus of Elasticity
Power CylindersMechanical PropertiesModerate Strength
PumpsCorrosion ResistanceCorrosion Resistance
PumpsMechanical PropertiesModerate Strength
SpringsCorrosion ResistanceCorrosion Resistance
SpringsMechanical PropertiesHigh Modulus of Elasticity
SpringsMechanical PropertiesModerate Strength
OrdnanceAmmunition ComponentsCorrosion ResistanceCorrosion Resistance
Ammunition ComponentsForming CharacteristicsFormability
Ammunition ComponentsMechanical PropertiesHigh Modulus of Elasticity
Ammunition ComponentsMechanical PropertiesModerate Strength
PlumbingPlumbing AccessoriesAppearanceAppearance
Plumbing AccessoriesCorrosion ResistanceCorrosion Resistance
Plumbing AccessoriesForming CharacteristicsFormability
Plumbing AccessoriesMechanical PropertiesModerate Strength
Plumbing Brass GoodsAppearanceAppearance
Plumbing Brass GoodsCorrosion ResistanceCorrosion Resistance
Plumbing Brass GoodsForming CharacteristicsFormability
Plumbing Brass GoodsMechanical PropertiesModerate Strength
Applicable Specifications
Form Application System Standard Description
CupsMILITARYMIL-C-10375CUPS, CASE, CARTRIDGE, COPPER ALLOY (FOR SMALL ARMS AMMUNITION)
Shim stockLaminateMILITARYMIL-S-22499SHIM STOCK, LAMINATED
Corrosion Properties

No information available.