Find suppliers for this alloy
C26200
| Elements | ||||
|---|---|---|---|---|
| Cu(1) | Pb | Zn | Fe | |
|
(1) Cu + Sum of Named Elements 99.7% min. |
||||
| Min (%) | 67.0 | |||
| Max (%) | 70.0 | 0.07 | Rem | 0.05 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Rockwell F scale | Rockwell 30T scale | Shear Strength (ksi) |
Fatigue Strength** (ksi) |
Section Size (in) |
Cold Work (%) |
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | ||||||||||||
| Flat Products | 1/2 Hard | H02 |
62 Typ |
52 Typ |
25 Typ |
70 Typ |
65 Typ |
40 Typ |
18 Typ | 0.04 | ||
| 1/4 Hard | H01 |
54 Typ |
40 Typ |
43 Typ |
55 Typ |
54 Typ |
36 Typ |
0.04 | ||||
| Extra Hard | H06 |
86 Typ |
65 Typ |
5 Typ |
88 Typ |
76 Typ |
46 Typ |
0.04 | ||||
| Extra Spring | H10 |
99 Typ |
65 Typ |
3 Typ |
93 Typ |
78 Typ |
0.04 | |||||
| Hard | H04 |
76 Typ |
63 Typ |
8 Typ |
82 Typ |
73 Typ |
44 Typ |
21 Typ | 0.04 | |||
| Nominal Grain Size 0.015 mm | OS015 |
53 Typ |
22 Typ |
54 Typ |
78 Typ |
43 Typ |
35 Typ |
0.04 | ||||
| Nominal Grain Size 0.025 mm | OS025 |
51 Typ |
19 Typ |
55 Typ |
72 Typ |
36 Typ |
0.04 | |||||
| Nominal Grain Size 0.035 mm | OS035 |
49 Typ |
17 Typ |
57 Typ |
68 Typ |
31 Typ |
34 Typ |
14 Typ | 0.04 | |||
| Nominal Grain Size 0.050 mm | OS050 |
47 Typ |
15 Typ |
62 Typ |
64 Typ |
26 Typ |
0.04 | |||||
| Nominal Grain Size 0.070 mm | OS070 |
46 Typ |
14 Typ |
65 Typ |
58 Typ |
15 Typ |
32 Typ |
13 Typ | 0.04 | |||
| Nominal Grain Size 0.100 mm | OS100 |
44 Typ |
11 Typ |
66 Typ |
54 Typ |
11 Typ |
13 Typ | 0.04 | ||||
| Spring | H08 |
94 Typ |
65 Typ |
3 Typ |
91 Typ |
77 Typ |
48 Typ |
23 Typ | 0.04 | |||
| Rod | 1/2 Hard | H02 |
70 Typ |
52 Typ |
330 Typ |
80 Typ |
42 Typ |
22 Typ | 1 | 20 | ||
| 1/8 Hard | H00 |
55 Typ |
40 Typ |
48 Typ |
60 Typ |
36 Typ |
1 | 6 | ||||
| Nominal Grain Size 0.050 mm | OS050 |
48 Typ |
16 Typ |
65 Typ |
65 Typ |
34 Typ |
1 | |||||
| Tube | Hard | H04 |
78 Typ |
64 Typ |
8 Typ |
82 Typ |
73 Typ |
35 | ||||
| Nominal Grain Size 0.025 mm | OS025 |
52 Typ |
20 Typ |
55 Typ |
75 Typ |
40 Typ |
||||||
| Nominal Grain Size 0.050 mm | OS050 |
47 Typ |
15 Typ |
65 Typ |
64 Typ |
26 Typ |
||||||
| Wire | 1/4 Hard | H01 |
70 Typ |
20 Typ |
0.08 | |||||||
| 1/8 Hard | H00 |
58 Typ |
35 Typ |
38 Typ |
0.08 | |||||||
| Extra Hard | H06 |
124 Typ |
4 Typ |
0.08 | ||||||||
| Nominal Grain Size 0.015 mm | OS015 |
54 Typ |
56 Typ |
0.08 | ||||||||
| Nominal Grain Size 0.025 mm | OS025 |
52 Typ |
58 Typ |
0.08 | ||||||||
| Nominal Grain Size 0.035 mm | OS035 |
50 Typ |
60 Typ |
34 Typ |
0.08 | |||||||
| Nominal Grain Size 0.050 mm | OS050 |
48 Typ |
64 Typ |
0.08 | ||||||||
| Spring | H08 |
130 Typ |
3 Typ |
60 Typ |
22 Typ | 0.08 | ||||||
| Melting Point - Liquidus°F | 1750 |
|---|---|
| Melting Point - Solidus°F | 1680 |
| Densitylb/cu in. at 68°F | 0.308 |
| Specific Gravity | 8.53 |
| Electrical Conductivity% IACS at 68°F | 28 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 70 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 11.1 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 16000 |
| Modulus of Rigidityksi | 6000 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Good |
| Gas Shielded Arc Welding | Fair |
| Coated Metal Arc Welding | Not Recommended |
| Spot Weld | Good |
| Seam Weld | Not Recommended |
| Butt Weld | Good |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Fair |
Common Fabrication Processes
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 800 | 1400 | ||
| Hot Working Temperature | 1350 | 1550 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Architecture | Grillwork | Appearance | Color |
| Grillwork | Corrosion Resistance | Corrosion Resistance | |
| Grillwork | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Grillwork | Forming Characteristics | Formability | |
| Grillwork | Mechanical Properties | Moderate Strength | |
| Automotive | Heater Cord | Corrosion Resistance | Corrosion Resistance |
| Heater Cord | Forming Characteristics | Formability | |
| Heater Cord | Mechanical Properties | Moderate Strength | |
| Radiators | Corrosion Resistance | Corrosion Resistance | |
| Radiators | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Radiators | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Radiators | Forming Characteristics | Formability | |
| Radiators | Mechanical Properties | Moderate Strength | |
| Radiators | Solderability | Solderability | |
| Tanks | Corrosion Resistance | Corrosion Resistance | |
| Tanks | Corrosion Resistance | Corrosion Resistance to Chemicals | |
| Tanks | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Tanks | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Tanks | Forming Characteristics | Formability | |
| Tanks | Mechanical Properties | Moderate Strength | |
| Tanks | Solderability | Solderability | |
| Tanks | Welding Characteristics | Weldability | |
| Builders Hardware | Finish Hardware | Corrosion Resistance | Corrosion Resistance |
| Finish Hardware | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Finish Hardware | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Finish Hardware | Forming Characteristics | Formability | |
| Finish Hardware | Mechanical Properties | Moderate Strength | |
| Hinges | Appearance | Color | |
| Hinges | Corrosion Resistance | Corrosion Resistance | |
| Hinges | Corrosion Resistance | Corrosion Resistance to Chemicals | |
| Hinges | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Hinges | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Hinges | Forming Characteristics | Formability | |
| Hinges | Mechanical Properties | Moderate Strength | |
| Kick Plates | Appearance | Color | |
| Kick Plates | Corrosion Resistance | Corrosion Resistance | |
| Kick Plates | Mechanical Properties | Moderate Strength | |
| Locks | Appearance | Color | |
| Locks | Corrosion Resistance | Corrosion Resistance | |
| Locks | Mechanical Properties | Moderate Strength | |
| Push Plates | Appearance | Color | |
| Push Plates | Corrosion Resistance | Corrosion Resistance | |
| Push Plates | Mechanical Properties | Moderate Strength | |
| Stencils | Forming Characteristics | Formability | |
| Stencils | Mechanical Properties | Moderate Strength | |
| Electrical | Flashlight Shells | Appearance | Color |
| Flashlight Shells | Corrosion Resistance | Corrosion Resistance | |
| Flashlight Shells | Forming Characteristics | Cold Workability | |
| Flashlight Shells | Forming Characteristics | Formability | |
| Flashlight Shells | Mechanical Properties | Moderate Strength | |
| Lamp Fixtures | Appearance | Color | |
| Lamp Fixtures | Corrosion Resistance | Corrosion Resistance | |
| Lamp Fixtures | Forming Characteristics | Formability | |
| Lamp Fixtures | Mechanical Properties | Moderate Strength | |
| Reflectors | Appearance | Color | |
| Reflectors | Corrosion Resistance | Corrosion Resistance | |
| Reflectors | Forming Characteristics | Formability | |
| Reflectors | Mechanical Properties | Moderate Strength | |
| Screw Shells | Corrosion Resistance | Corrosion Resistance | |
| Screw Shells | Forming Characteristics | Formability | |
| Screw Shells | Mechanical Properties | Moderate Strength | |
| Socket Shells | Corrosion Resistance | Corrosion Resistance | |
| Socket Shells | Forming Characteristics | Formability | |
| Fasteners | Eyelets | Appearance | Color |
| Eyelets | Corrosion Resistance | Corrosion Resistance | |
| Eyelets | Forming Characteristics | Formability | |
| Eyelets | Mechanical Properties | Moderate Strength | |
| Fasteners | Conductivity (Electrical) | Electrical Conductivity | |
| Fasteners | Corrosion Resistance | Corrosion Resistance | |
| Fasteners | Mechanical Properties | Moderate to High Strength | |
| Fasteners for Electrical | Conductivity (Electrical) | Electrical Conductivity | |
| Fasteners for Electrical | Corrosion Resistance | Corrosion Resistance | |
| Fasteners for Electrical | Mechanical Properties | Moderate to High Strength | |
| Grommets | Appearance | Color | |
| Grommets | Corrosion Resistance | Corrosion Resistance | |
| Grommets | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Grommets | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Grommets | Forming Characteristics | Formability | |
| Grommets | Mechanical Properties | Moderate Strength | |
| Pins | Appearance | Color | |
| Pins | Corrosion Resistance | Corrosion Resistance | |
| Pins | Forming Characteristics | Formability | |
| Pins | Mechanical Properties | Moderate Strength | |
| Rivets | Appearance | Color | |
| Rivets | Corrosion Resistance | Corrosion Resistance | |
| Rivets | Forming Characteristics | Formability | |
| Rivets | Mechanical Properties | Moderate Strength | |
| Screws | Corrosion Resistance | Corrosion Resistance | |
| Screws | Corrosion Resistance | Corrosion Resistance to Chemicals | |
| Screws | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Screws | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Screws | Forming Characteristics | Formability | |
| Screws | Mechanical Properties | Moderate Strength | |
| Industrial | Bead Chain | Appearance | Color |
| Bead Chain | Corrosion Resistance | Corrosion Resistance | |
| Bead Chain | Forming Characteristics | Formability | |
| Bead Chain | Mechanical Properties | Moderate Strength | |
| Chain | Appearance | Color | |
| Chain | Corrosion Resistance | Corrosion Resistance | |
| Chain | Forming Characteristics | Formability | |
| Chain | Mechanical Properties | Moderate Strength | |
| Liners | Corrosion Resistance | Corrosion Resistance | |
| Liners | Corrosion Resistance | Corrosion Resistance to Chemicals | |
| Liners | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Liners | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Liners | Forming Characteristics | Formability | |
| Liners | Mechanical Properties | Moderate Strength | |
| Power Cylinders | Corrosion Resistance | Corrosion Resistance | |
| Power Cylinders | Corrosion Resistance | Corrosion Resistance to Chemicals | |
| Power Cylinders | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Power Cylinders | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Power Cylinders | Forming Characteristics | Cold Workability | |
| Power Cylinders | Mechanical Properties | Moderate Strength | |
| Pumps | Corrosion Resistance | Corrosion Resistance | |
| Pumps | Corrosion Resistance | Corrosion Resistance to Chemicals | |
| Pumps | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Pumps | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Pumps | Forming Characteristics | Formability | |
| Pumps | Mechanical Properties | Moderate Strength | |
| Springs | Corrosion Resistance | Corrosion Resistance | |
| Springs | Forming Characteristics | Formability | |
| Springs | Mechanical Properties | High Modulus of Elasticity | |
| Springs | Mechanical Properties | High Strength | |
| Ordnance | Ammunition Components | Mechanical Properties | High Modulus of Elasticity |
| Ammunition Components | Mechanical Properties | Moderate Strength | |
| Plumbing | Plumbing Accessories | Appearance | Color |
| Plumbing Accessories | Corrosion Resistance | Corrosion Resistance | |
| Plumbing Accessories | Forming Characteristics | Formability | |
| Plumbing Accessories | Mechanical Properties | Moderate Strength | |
| Plumbing Brass Goods | Appearance | Color | |
| Plumbing Brass Goods | Corrosion Resistance | Corrosion Resistance | |
| Plumbing Brass Goods | Forming Characteristics | Formability | |
| Plumbing Brass Goods | Mechanical Properties | Moderate Strength |
Applicable Specifications
Corrosion Properties