Chemical Composition
Element
Cu(1)PbZnFe
(1) Cu + Sum of Named Elements 99.7% min.
Min (%)67.0
Max (%)70.00.07Rem0.05
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell F scale
Rockwell 30T scale
Shear Strength
(ksi)
Fatigue Strength**
(ksi)
Section Size
(in)
Cold Work
(%)
Flat Products1/2 HardH0262   Typ
52   Typ
25   Typ
70   Typ
65   Typ
40   Typ
18   Typ
0.04
1/4 HardH0154   Typ
40   Typ
43   Typ
55   Typ
54   Typ
36   Typ
0.04
Extra HardH0686   Typ
65   Typ
5   Typ
88   Typ
76   Typ
46   Typ
0.04
Extra SpringH1099   Typ
65   Typ
3   Typ
93   Typ
78   Typ
0.04
HardH0476   Typ
63   Typ
8   Typ
82   Typ
73   Typ
44   Typ
21   Typ
0.04
Nominal Grain Size 0.015 mmOS01553   Typ
22   Typ
54   Typ
78   Typ
43   Typ
35   Typ
0.04
Nominal Grain Size 0.025 mmOS02551   Typ
19   Typ
55   Typ
72   Typ
36   Typ
0.04
Nominal Grain Size 0.035 mmOS03549   Typ
17   Typ
57   Typ
68   Typ
31   Typ
34   Typ
14   Typ
0.04
Nominal Grain Size 0.050 mmOS05047   Typ
15   Typ
62   Typ
64   Typ
26   Typ
0.04
Nominal Grain Size 0.070 mmOS07046   Typ
14   Typ
65   Typ
58   Typ
15   Typ
32   Typ
13   Typ
0.04
Nominal Grain Size 0.100 mmOS10044   Typ
11   Typ
66   Typ
54   Typ
11   Typ
13   Typ
0.04
SpringH0894   Typ
65   Typ
3   Typ
91   Typ
77   Typ
48   Typ
23   Typ
0.04
Rod1/2 HardH0270   Typ
52   Typ
330   Typ
80   Typ
42   Typ
22   Typ
120
1/8 HardH0055   Typ
40   Typ
48   Typ
60   Typ
36   Typ
16
Nominal Grain Size 0.050 mmOS05048   Typ
16   Typ
65   Typ
65   Typ
34   Typ
1
TubeHardH0478   Typ
64   Typ
8   Typ
82   Typ
73   Typ
35
Nominal Grain Size 0.025 mmOS02552   Typ
20   Typ
55   Typ
75   Typ
40   Typ
Nominal Grain Size 0.050 mmOS05047   Typ
15   Typ
65   Typ
64   Typ
26   Typ
Wire1/4 HardH0170   Typ
20   Typ
0.08
1/8 HardH0058   Typ
35   Typ
38   Typ
0.08
Extra HardH06124   Typ
4   Typ
0.08
Nominal Grain Size 0.015 mmOS01554   Typ
56   Typ
0.08
Nominal Grain Size 0.025 mmOS02552   Typ
58   Typ
0.08
Nominal Grain Size 0.035 mmOS03550   Typ
60   Typ
34   Typ
0.08
Nominal Grain Size 0.050 mmOS05048   Typ
64   Typ
0.08
SpringH08130   Typ
3   Typ
60   Typ
22   Typ
0.08
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
Melting Point - Liquidus°F1750
Melting Point - Solidus°F1680
Densitylb/cu in. at 68°F0.308
Specific Gravity8.53
Electrical Conductivity% IACS at 68°F28
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F70
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)11.1
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi16000
Modulus of Rigidityksi6000
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingGood
Gas Shielded Arc WeldingFair
Coated Metal Arc WeldingNot Recommended
Spot WeldGood
Seam WeldNot Recommended
Butt WeldGood
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedFair
Fabrication Process Properties

No fabrication process properties for this alloy

    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing8001400
Hot Treatment13501550
Typical uses
Product Category Product Reason Category Reason
ArchitectureGrillworkAppearanceColor
GrillworkCorrosion ResistanceCorrosion Resistance
GrillworkCorrosion ResistanceCorrosion Resistance to Fresh Water
GrillworkForming CharacteristicsFormability
GrillworkMechanical PropertiesModerate Strength
AutomotiveHeater CordCorrosion ResistanceCorrosion Resistance
Heater CordForming CharacteristicsFormability
Heater CordMechanical PropertiesModerate Strength
RadiatorsCorrosion ResistanceCorrosion Resistance
RadiatorsCorrosion ResistanceCorrosion Resistance to Fresh Water
RadiatorsCorrosion ResistanceCorrosion Resistance to Salt Water
RadiatorsForming CharacteristicsFormability
RadiatorsMechanical PropertiesModerate Strength
RadiatorsSolderabilitySolderability
TanksCorrosion ResistanceCorrosion Resistance
TanksCorrosion ResistanceCorrosion Resistance to Chemicals
TanksCorrosion ResistanceCorrosion Resistance to Fresh Water
TanksCorrosion ResistanceCorrosion Resistance to Salt Water
TanksForming CharacteristicsFormability
TanksMechanical PropertiesModerate Strength
TanksSolderabilitySolderability
TanksWelding CharacteristicsWeldability
Builders HardwareFinish HardwareCorrosion ResistanceCorrosion Resistance
Finish HardwareCorrosion ResistanceCorrosion Resistance to Fresh Water
Finish HardwareCorrosion ResistanceCorrosion Resistance to Salt Water
Finish HardwareForming CharacteristicsFormability
Finish HardwareMechanical PropertiesModerate Strength
HingesAppearanceColor
HingesCorrosion ResistanceCorrosion Resistance
HingesCorrosion ResistanceCorrosion Resistance to Chemicals
HingesCorrosion ResistanceCorrosion Resistance to Fresh Water
HingesCorrosion ResistanceCorrosion Resistance to Salt Water
HingesForming CharacteristicsFormability
HingesMechanical PropertiesModerate Strength
Kick PlatesAppearanceColor
Kick PlatesCorrosion ResistanceCorrosion Resistance
Kick PlatesMechanical PropertiesModerate Strength
LocksAppearanceColor
LocksCorrosion ResistanceCorrosion Resistance
LocksMechanical PropertiesModerate Strength
Push PlatesAppearanceColor
Push PlatesCorrosion ResistanceCorrosion Resistance
Push PlatesMechanical PropertiesModerate Strength
StencilsForming CharacteristicsFormability
StencilsMechanical PropertiesModerate Strength
ElectricalFlashlight ShellsAppearanceColor
Flashlight ShellsCorrosion ResistanceCorrosion Resistance
Flashlight ShellsForming CharacteristicsCold Workability
Flashlight ShellsForming CharacteristicsFormability
Flashlight ShellsMechanical PropertiesModerate Strength
Lamp FixturesAppearanceColor
Lamp FixturesCorrosion ResistanceCorrosion Resistance
Lamp FixturesForming CharacteristicsFormability
Lamp FixturesMechanical PropertiesModerate Strength
ReflectorsAppearanceColor
ReflectorsCorrosion ResistanceCorrosion Resistance
ReflectorsForming CharacteristicsFormability
ReflectorsMechanical PropertiesModerate Strength
Screw ShellsCorrosion ResistanceCorrosion Resistance
Screw ShellsForming CharacteristicsFormability
Screw ShellsMechanical PropertiesModerate Strength
Socket ShellsCorrosion ResistanceCorrosion Resistance
Socket ShellsForming CharacteristicsFormability
FastenersEyeletsAppearanceColor
EyeletsCorrosion ResistanceCorrosion Resistance
EyeletsForming CharacteristicsFormability
EyeletsMechanical PropertiesModerate Strength
FastenersConductivity (Electrical)Electrical Conductivity
FastenersCorrosion ResistanceCorrosion Resistance
FastenersMechanical PropertiesModerate to High Strength
Fasteners for ElectricalConductivity (Electrical)Electrical Conductivity
Fasteners for ElectricalCorrosion ResistanceCorrosion Resistance
Fasteners for ElectricalMechanical PropertiesModerate to High Strength
GrommetsAppearanceColor
GrommetsCorrosion ResistanceCorrosion Resistance
GrommetsCorrosion ResistanceCorrosion Resistance to Fresh Water
GrommetsCorrosion ResistanceCorrosion Resistance to Salt Water
GrommetsForming CharacteristicsFormability
GrommetsMechanical PropertiesModerate Strength
PinsAppearanceColor
PinsCorrosion ResistanceCorrosion Resistance
PinsForming CharacteristicsFormability
PinsMechanical PropertiesModerate Strength
RivetsAppearanceColor
RivetsCorrosion ResistanceCorrosion Resistance
RivetsForming CharacteristicsFormability
RivetsMechanical PropertiesModerate Strength
ScrewsCorrosion ResistanceCorrosion Resistance
ScrewsCorrosion ResistanceCorrosion Resistance to Chemicals
ScrewsCorrosion ResistanceCorrosion Resistance to Fresh Water
ScrewsCorrosion ResistanceCorrosion Resistance to Salt Water
ScrewsForming CharacteristicsFormability
ScrewsMechanical PropertiesModerate Strength
IndustrialBead ChainAppearanceColor
Bead ChainCorrosion ResistanceCorrosion Resistance
Bead ChainForming CharacteristicsFormability
Bead ChainMechanical PropertiesModerate Strength
ChainAppearanceColor
ChainCorrosion ResistanceCorrosion Resistance
ChainForming CharacteristicsFormability
ChainMechanical PropertiesModerate Strength
LinersCorrosion ResistanceCorrosion Resistance
LinersCorrosion ResistanceCorrosion Resistance to Chemicals
LinersCorrosion ResistanceCorrosion Resistance to Fresh Water
LinersCorrosion ResistanceCorrosion Resistance to Salt Water
LinersForming CharacteristicsFormability
LinersMechanical PropertiesModerate Strength
Power CylindersCorrosion ResistanceCorrosion Resistance
Power CylindersCorrosion ResistanceCorrosion Resistance to Chemicals
Power CylindersCorrosion ResistanceCorrosion Resistance to Fresh Water
Power CylindersCorrosion ResistanceCorrosion Resistance to Salt Water
Power CylindersForming CharacteristicsCold Workability
Power CylindersMechanical PropertiesModerate Strength
PumpsCorrosion ResistanceCorrosion Resistance
PumpsCorrosion ResistanceCorrosion Resistance to Chemicals
PumpsCorrosion ResistanceCorrosion Resistance to Fresh Water
PumpsCorrosion ResistanceCorrosion Resistance to Salt Water
PumpsForming CharacteristicsFormability
PumpsMechanical PropertiesModerate Strength
SpringsCorrosion ResistanceCorrosion Resistance
SpringsForming CharacteristicsFormability
SpringsMechanical PropertiesHigh Modulus of Elasticity
SpringsMechanical PropertiesHigh Strength
OrdnanceAmmunition ComponentsMechanical PropertiesHigh Modulus of Elasticity
Ammunition ComponentsMechanical PropertiesModerate Strength
PlumbingPlumbing AccessoriesAppearanceColor
Plumbing AccessoriesCorrosion ResistanceCorrosion Resistance
Plumbing AccessoriesForming CharacteristicsFormability
Plumbing AccessoriesMechanical PropertiesModerate Strength
Plumbing Brass GoodsAppearanceColor
Plumbing Brass GoodsCorrosion ResistanceCorrosion Resistance
Plumbing Brass GoodsForming CharacteristicsFormability
Plumbing Brass GoodsMechanical PropertiesModerate Strength
Applicable Specifications

No applicable specifications for this alloy

Corrosion Properties

No information available.