Find suppliers for this alloyC26800
Chemical Composition
Element
Cu(1)PbZnFe
(1) Cu + Sum of Named Elements 99.7% min.
Min (%)64.0
Max (%)68.50.09Rem0.05
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell F scale
Rockwell 30T scale
Shear Strength
(ksi)
Fatigue Strength**
(ksi)
Section Size
(in)
Cold Work
(%)
Flat Products1/2 HardH0261   Typ
50   Typ
23   Typ
70   Typ
65   Typ
40   Typ
0.04
1/4 HardH0154   Typ
40   Typ
43   Typ
55   Typ
54   Typ
36   Typ
0.04
1/8 HardH0050   Typ
35   Typ
50   Typ
50   Typ
50   Typ
0.04
Extra HardH0685   Typ
62   Typ
5   Typ
87   Typ
74   Typ
45   Typ
0.04
HardH0474   Typ
60   Typ
8   Typ
80   Typ
70   Typ
43   Typ
14   Typ
0.04
Nominal Grain Size 0.015 mmOS01553   Typ
22   Typ
54   Typ
78   Typ
43   Typ
0.04
Nominal Grain Size 0.025 mmOS02551   Typ
19   Typ
55   Typ
72   Typ
36   Typ
0.04
Nominal Grain Size 0.035 mmOS03549   Typ
17   Typ
57   Typ
68   Typ
31   Typ
34   Typ
0.04
Nominal Grain Size 0.050 mmOS05047   Typ
15   Typ
62   Typ
64   Typ
26   Typ
0.04
Nominal Grain Size 0.070 mmOS07046   Typ
14   Typ
65   Typ
58   Typ
15   Typ
32   Typ
12   Typ
0.04
SpringH0891   Typ
62   Typ
3   Typ
90   Typ
76   Typ
47   Typ
20   Typ
0.04
Rod1/8 HardH0055   Typ
40   Typ
48   Typ
55   Typ
36   Typ
16
Nominal Grain Size 0.050 mmOS05048   Typ
16   Typ
65   Typ
65   Typ
34   Typ
1
Wire1/2 HardH0288   Typ
15   Typ
0.08
1/4 HardH0170   Typ
20   Typ
42   Typ
22   Typ
0.08
1/8 HardH0058   Typ
35   Typ
38   Typ
0.08
Extra HardH06120   Typ
4   Typ
60   Typ
0.08
HardH04110   Typ
8   Typ
55   Typ
0.08
Nominal Grain Size 0.035 mmOS03550   Typ
60   Typ
34   Typ
0.08
SpringH08128   Typ
3   Typ
60   Typ
0.08
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
Melting Point - Liquidus°F1710
Melting Point - Solidus°F1660
Densitylb/cu in. at 68°F0.306
Specific Gravity8.47
Electrical Conductivity% IACS at 68°F27
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F67
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)11.3
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi15000
Modulus of Rigidityksi5600
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingGood
Gas Shielded Arc WeldingFair
Coated Metal Arc WeldingNot Recommended
Spot WeldGood
Seam WeldNot Recommended
Butt WeldGood
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedPoor
Machinability Rating30
Common Fabrication Processes
  • Blanking
  • Drawing
  • Etching
  • Forming and Bending
  • Heading and Upsetting
  • Piercing and Punching
  • Roll Threading and Knurling
  • Shearing
  • Spinning
  • Squeezing and Swaging
  • Stamping
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing8001300
Typical uses
Product Category Product Reason Category Reason
ArchitectureGrillworkAppearanceColor
GrillworkCorrosion ResistanceCorrosion Resistance
GrillworkMechanical PropertiesModerate Strength
HandrailsAppearanceColor
AutomotiveRadiator CoresCorrosion ResistanceCorrosion Resistance
Radiator CoresForming CharacteristicsFormability
Radiator CoresMechanical PropertiesModerate Strength
Radiator CoresSolderabilitySolderability
TanksCorrosion ResistanceCorrosion Resistance
TanksForming CharacteristicsFormability
TanksMechanical PropertiesModerate Strength
TanksSolderabilitySolderability
Builders HardwareFinish HardwareAppearanceColor
Finish HardwareCorrosion ResistanceCorrosion Resistance
Finish HardwareForming CharacteristicsFormability
Finish HardwareMechanical PropertiesModerate Strength
HingesAppearanceColor
HingesCorrosion ResistanceCorrosion Resistance
HingesForming CharacteristicsFormability
HingesMechanical PropertiesModerate Strength
Kick PlatesAppearanceColor
Kick PlatesCorrosion ResistanceCorrosion Resistance
Kick PlatesMechanical PropertiesModerate Strength
LocksAppearanceColor
LocksCorrosion ResistanceCorrosion Resistance
LocksForming CharacteristicsFormability
LocksMechanical PropertiesModerate Strength
Push PlatesAppearanceColor
Push PlatesCorrosion ResistanceCorrosion Resistance
Push PlatesMechanical PropertiesModerate Strength
StencilsAppearanceColor
StencilsCorrosion ResistanceCorrosion Resistance
StencilsMechanical PropertiesModerate Strength
ElectricalClipsCorrosion ResistanceCorrosion Resistance
ClipsForming CharacteristicsFormability
ClipsMechanical PropertiesHigh Strength
Flashlight ShellsCorrosion ResistanceCorrosion Resistance
Flashlight ShellsForming CharacteristicsCold Workability
Flashlight ShellsForming CharacteristicsFormability
Flashlight ShellsMechanical PropertiesModerate Strength
Lamp FixturesAppearanceColor
Lamp FixturesCorrosion ResistanceCorrosion Resistance
Lamp FixturesForming CharacteristicsFormability
Lamp FixturesMechanical PropertiesModerate Strength
Lamp SocketsAppearanceAppearance
Lamp SocketsCorrosion ResistanceCorrosion Resistance
Lamp SocketsForming CharacteristicsFormability
Lamp SocketsMechanical PropertiesHigh Strength
ReflectorsAppearanceColor
ReflectorsCorrosion ResistanceCorrosion Resistance
ReflectorsForming CharacteristicsFormability
ReflectorsMechanical PropertiesModerate Strength
Screw ShellsAppearanceColor
Screw ShellsCorrosion ResistanceCorrosion Resistance
Screw ShellsForming CharacteristicsCold Workability
Screw ShellsForming CharacteristicsFormability
Screw ShellsMechanical PropertiesModerate Strength
Socket ShellsCorrosion ResistanceCorrosion Resistance
Socket ShellsForming CharacteristicsFormability
Socket ShellsMechanical PropertiesModerate Strength
WireCorrosion ResistanceCorrosion Resistance
WireForming CharacteristicsCold Workability
WireMechanical PropertiesHigh Strength
WireMechanical PropertiesModerate Strength
FastenersEyeletsAppearanceColor
EyeletsCorrosion ResistanceCorrosion Resistance
EyeletsForming CharacteristicsFormability
EyeletsMechanical PropertiesModerate Strength
FastenersConductivity (Electrical)Electrical Conductivity
FastenersCorrosion ResistanceCorrosion Resistance
GrommetsAppearanceColor
GrommetsCorrosion ResistanceCorrosion Resistance
GrommetsForming CharacteristicsFormability
GrommetsMechanical PropertiesModerate Strength
PinsCorrosion ResistanceCorrosion Resistance
PinsForming CharacteristicsFormability
PinsMechanical PropertiesModerate Strength
RivetsAppearanceColor
RivetsCorrosion ResistanceCorrosion Resistance
RivetsForming CharacteristicsFormability
RivetsMechanical PropertiesModerate Strength
ScrewsCorrosion ResistanceCorrosion Resistance
ScrewsForming CharacteristicsFormability
ScrewsMechanical PropertiesModerate Strength
IndustrialAir Pressure Conveyer SystemsCorrosion ResistanceCorrosion Resistance
Air Pressure Conveyer SystemsForming CharacteristicsFormability
Air Pressure Conveyer SystemsMechanical PropertiesHigh Strength
Air Pressure Conveyer SystemsPressure TightPressure Tight
Bead ChainCorrosion ResistanceCorrosion Resistance
Bead ChainForming CharacteristicsFormability
Bead ChainMechanical PropertiesModerate Strength
ChainAppearanceColor
ChainCorrosion ResistanceCorrosion Resistance
ChainForming CharacteristicsFormability
ChainMechanical PropertiesModerate Strength
SpringsCorrosion ResistanceCorrosion Resistance
SpringsForming CharacteristicsFormability
SpringsMechanical PropertiesHigh Modulus of Elasticity
SpringsMechanical PropertiesHigh Strength
MarineFastenersConductivity (Electrical)Electrical Conductivity
FastenersCorrosion ResistanceCorrosion Resistance
PlumbingBathroom FixturesAppearanceColor
Bathroom FixturesCorrosion ResistanceCorrosion Resistance
Bathroom FixturesForming CharacteristicsFormability
Bathroom FixturesMechanical PropertiesModerate Strength
Plumbing AccessoriesAppearanceColor
Plumbing AccessoriesCorrosion ResistanceCorrosion Resistance
Plumbing AccessoriesForming CharacteristicsFormability
Plumbing AccessoriesMechanical PropertiesModerate Strength
Sanitary TrapsCorrosion ResistanceCorrosion Resistance
Sanitary TrapsForming CharacteristicsFormability
Sanitary TrapsMechanical PropertiesModerate Strength
Sink StrainersAppearanceColor
Sink StrainersCorrosion ResistanceCorrosion Resistance
Sink StrainersForming CharacteristicsFormability
Sink StrainersMechanical PropertiesModerate Strength
Applicable Specifications
Form Specific Sub-Form System Standard Description
BarASTMB36/B36MBRASS PLATE, SHEET, STRIP AND ROLLED BAR
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
PlateASTMB36/B36MBRASS PLATE, SHEET, STRIP AND ROLLED BAR
RodSAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
Rod, Bar & ShapesASTMB927/B927MBRASS ROD, BAR, AND SHAPES
SheetASTMB36/B36MBRASS PLATE, SHEET, STRIP AND ROLLED BAR
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
StripASTMB36/B36MBRASS PLATE, SHEET, STRIP AND ROLLED BAR
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
TubeWeldedASTMB587WELDED BRASS TUBE
WireMetallizingMILITARYMIL-W-6712WIRE, METALLIZING
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
Corrosion Properties

No information available.