Find suppliers for this alloyC27000
Chemical Composition
Element
Cu(1)PbZnFe
(1) Cu + Sum of Named Elements 99.7% min.
Min (%)63.0
Max (%)68.50.09Rem0.07
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell F scale
Rockwell 30T scale
Shear Strength
(ksi)
Torsion Modulus
(ksi)
Fatigue Strength**
(ksi)
Ultimate Tensile Strength in Shear
(ksi)
Section Size
(in)
Cold Work
(%)
Flat Products1/2 HardH0261   Typ
50   Typ
23   Typ
70   Typ
65   Typ
40   Typ
0.04
1/4 HardH0154   Typ
40   Typ
43   Typ
55   Typ
54   Typ
36   Typ
0.04
1/8 HardH0050   Typ
35   Typ
50   Typ
50   Typ
50   Typ
0.04
Extra HardH0685   Typ
62   Typ
5   Typ
87   Typ
74   Typ
45   Typ
0.04
HardH0474   Typ
60   Typ
8   Typ
80   Typ
70   Typ
43   Typ
14   Typ
0.04
Nominal Grain Size 0.015 mmOS01553   Typ
22   Typ
54   Typ
78   Typ
43   Typ
0.04
Nominal Grain Size 0.025 mmOS02551   Typ
19   Typ
55   Typ
72   Typ
36   Typ
0.04
Nominal Grain Size 0.035 mmOS03549   Typ
17   Typ
57   Typ
68   Typ
31   Typ
34   Typ
0.04
Nominal Grain Size 0.050 mmOS05047   Typ
15   Typ
62   Typ
64   Typ
26   Typ
0.04
Nominal Grain Size 0.070 mmOS07046   Typ
14   Typ
65   Typ
32   Typ
0.04
OS07046   Typ
14   Typ
65   Typ
58   Typ
15   Typ
32   Typ
12   Typ
0.04
SpringH0891   Typ
62   Typ
3   Typ
90   Typ
76   Typ
47   Typ
20   Typ
0.04
Rod1/8 HardH0055   Typ
40   Typ
48   Typ
55   Typ
36   Typ
5.1   Typ
16
Nominal Grain Size 0.050 mmOS05048   Typ
16   Typ
65   Typ
65   Typ
34   Typ
1
Wire1/2 HardH0288   Typ
15   Typ
0.08
1/4 HardH0170   Typ
57   Typ
20   Typ
22   Typ
42   Typ
0.08
1/8 HardH0058   Typ
35   Typ
38   Typ
0.08
Extra HardH06120   Typ
4   Typ
60   Typ
0.08
HardH04110   Typ
8   Typ
55   Typ
0.08
Nominal Grain Size 0.035 mmOS03550   Typ
60   Typ
34   Typ
0.08
SpringH08128   Typ
3   Typ
60   Typ
0.08
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
Melting Point - Liquidus°F1710
Melting Point - Solidus°F1660
Densitylb/cu in. at 68°F0.306
Specific Gravity8.47
Electrical Conductivity% IACS at 68°F27
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F67
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)11.3
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi15000
Modulus of Rigidityksi5600
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingGood
Gas Shielded Arc WeldingFair
Coated Metal Arc WeldingNot Recommended
Spot WeldGood
Seam WeldNot Recommended
Butt WeldGood
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedPoor
Machinability Rating30
Common Fabrication Processes
  • Blanking
  • Drawing
  • Etching
  • Forming and Bending
  • Heading and Upsetting
  • Piercing and Punching
  • Roll Threading and Knurling
  • Shearing
  • Spinning
  • Squeezing and Swaging
  • Stamping
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing8001300
Typical uses
Product Category Product Reason Category Reason
ArchitectureGrillworkAppearanceAppearance
GrillworkAppearanceColor
GrillworkCorrosion ResistanceCorrosion Resistance
HandrailsAppearanceColor
HandrailsConductivity (Thermal)Thermal Conductivity
HandrailsForming CharacteristicsFormability
AutomotiveRadiator CoresAppearanceAppearance
Radiator CoresCorrosion ResistanceCorrosion Resistance
Radiator CoresForming CharacteristicsCold Workability
Radiator CoresForming CharacteristicsFormability
Radiator CoresMechanical PropertiesModerate Strength
TanksAppearanceAppearance
TanksCorrosion ResistanceCorrosion Resistance
TanksMechanical PropertiesModerate Strength
Builders HardwareFinish HardwareAppearanceAppearance
Finish HardwareAppearanceColor
Finish HardwareCorrosion ResistanceCorrosion Resistance
HingesAppearanceAppearance
HingesAppearanceColor
HingesCorrosion ResistanceCorrosion Resistance
HingesMechanical PropertiesModerate Strength
Kick PlatesAppearanceAppearance
Kick PlatesAppearanceColor
Kick PlatesCorrosion ResistanceCorrosion Resistance
Kick PlatesMechanical PropertiesModerate Strength
LocksAppearanceAppearance
LocksCorrosion ResistanceCorrosion Resistance
LocksForming CharacteristicsFormability
LocksMechanical PropertiesModerate Strength
Push PlatesAppearanceAppearance
Push PlatesCorrosion ResistanceCorrosion Resistance
Push PlatesMechanical PropertiesModerate Strength
StencilsAppearanceAppearance
StencilsCorrosion ResistanceCorrosion Resistance
StencilsMechanical PropertiesModerate Strength
ElectricalFlashlight ShellsAppearanceAppearance
Flashlight ShellsAppearanceColor
Flashlight ShellsCorrosion ResistanceCorrosion Resistance
Flashlight ShellsForming CharacteristicsCold Workability
Lamp FixturesAppearanceColor
Lamp FixturesCorrosion ResistanceCorrosion Resistance
Lamp FixturesForming CharacteristicsFormability
Lamp FixturesMechanical PropertiesModerate Strength
ReflectorsAppearanceAppearance
ReflectorsCorrosion ResistanceCorrosion Resistance
ReflectorsMechanical PropertiesModerate Strength
Screw ShellsAppearanceAppearance
Screw ShellsCorrosion ResistanceCorrosion Resistance
Screw ShellsForming CharacteristicsFormability
Screw ShellsMechanical PropertiesModerate Strength
Socket ShellsAppearanceAppearance
Socket ShellsCorrosion ResistanceCorrosion Resistance
Socket ShellsForming CharacteristicsCold Workability
Socket ShellsForming CharacteristicsFormability
Socket ShellsMechanical PropertiesModerate Strength
FastenersEyeletsAppearanceColor
EyeletsCorrosion ResistanceCorrosion Resistance
EyeletsForming CharacteristicsFormability
EyeletsMechanical PropertiesModerate Strength
FastenersConductivity (Electrical)Electrical Conductivity
FastenersCorrosion ResistanceCorrosion Resistance
FastenersMechanical PropertiesModerate Strength
GrommetsAppearanceAppearance
GrommetsAppearanceColor
GrommetsCorrosion ResistanceCorrosion Resistance
GrommetsForming CharacteristicsFormability
GrommetsMechanical PropertiesModerate Strength
PinsAppearanceAppearance
PinsCorrosion ResistanceCorrosion Resistance
PinsMechanical PropertiesModerate Strength
RivetsAppearanceAppearance
RivetsCorrosion ResistanceCorrosion Resistance
RivetsForming CharacteristicsFormability
RivetsMechanical PropertiesModerate Strength
ScrewsAppearanceAppearance
ScrewsCorrosion ResistanceCorrosion Resistance
ScrewsMechanical PropertiesModerate Strength
IndustrialBead ChainAppearanceColor
Bead ChainCorrosion ResistanceCorrosion Resistance
Bead ChainForming CharacteristicsFormability
Bead ChainMechanical PropertiesModerate Strength
ChainAppearanceColor
ChainCorrosion ResistanceCorrosion Resistance
ChainForming CharacteristicsFormability
ChainMechanical PropertiesModerate Strength
SpringsCorrosion ResistanceCorrosion Resistance
SpringsMechanical PropertiesHigh Modulus of Elasticity
SpringsMechanical PropertiesModerate Strength
MarineFastenersConductivity (Electrical)Electrical Conductivity
FastenersCorrosion ResistanceCorrosion Resistance
FastenersMechanical PropertiesModerate Strength
PlumbingPlumbing AccessoriesAppearanceAppearance
Plumbing AccessoriesCorrosion ResistanceCorrosion Resistance
Plumbing AccessoriesForming CharacteristicsCold Workability
Plumbing AccessoriesForming CharacteristicsFormability
Plumbing AccessoriesMechanical PropertiesModerate Strength
Sink StrainersAppearanceAppearance
Sink StrainersCorrosion ResistanceCorrosion Resistance
Sink StrainersMechanical PropertiesModerate Strength
Applicable Specifications
Form Sub-Form Specific Sub-Form System Standard Description
BoltsASTMF468NONFERROUS BOLTS, HEX CAP SCREWS, AND STUDS FOR GENERAL USE
NutsASTMF467NONFERROUS NUTS FOR GENERAL USE
RodSAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
Rod, Bar & ShapesASTMB927/B927MBRASS ROD, BAR, AND SHAPES
ScrewsASTMF468NONFERROUS BOLTS, HEX CAP SCREWS, AND STUDS FOR GENERAL USE
StudsASTMF468NONFERROUS BOLTS, HEX CAP SCREWS, AND STUDS FOR GENERAL USE
TubeSeamlessASMESB135SEAMLESS BRASS TUBE
ASTMB135Tube, Seamless
Seamless (Metric)ASTMB135/B135MSeamless Brass Tube
WeldedASTMB587WELDED BRASS TUBE
WireCoated With TinAMS4710BRASS WIRE, TINNED, ANNEALED
AMS4712BRASS WIRE, ANNEALED
AMS4713WIRE, BRASS, EIGHTH-HARD
ASTMB134/B134MBRASS WIRE
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
Corrosion Properties

No information available.