Find suppliers for this alloy
C27200
| Elements | ||||
|---|---|---|---|---|
| Cu(1) | Pb | Zn | Fe | |
|
(1) Cu + Sum of Named Elements 99.7% min. |
||||
| Min (%) | 62.0 | |||
| Max (%) | 65.0 | 0.07 | Rem | 0.07 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell F scale | Section Size (in) |
|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||||
| Tube | Hard Drawn | H80 |
74 Typ |
55 Typ |
10 Typ |
80 Typ |
0.065 |
| Nominal Grain Size 0.025 mm | OS025 |
56 Typ |
23 Typ |
50 Typ |
82 Typ |
0.065 | |
| Melting Point - Liquidus°F | 1680 |
|---|---|
| Densitylb/cu in. at 68°F | 0.305 |
| Specific Gravity | 8.44 |
| Electrical Conductivity% IACS at 68°F | 27.6 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 67 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 11.4 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 15000 |
| Modulus of Rigidityksi | 5600 |
Fabrication Properties
Common Fabrication Processes
- Drawing
- Forming and Bending
- Shearing
- Spinning
- Swaging
Thermal Properties
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Fasteners | Fasteners | Corrosion Resistance | Corrosion Resistance |
| Fasteners | Forming Characteristics | Formability | |
| Fasteners | Mechanical Properties | Moderate Strength | |
| Industrial | Cold Headed Parts | Conductivity (Electrical) | Electrical Conductivity |
| Cold Headed Parts | Conductivity (Thermal) | Thermal Conductivity | |
| Cold Headed Parts | Corrosion Resistance | Corrosion Resistance | |
| Cold Headed Parts | Forming Characteristics | Formability | |
| Heat Exchanger Shells | Corrosion Resistance | Corrosion Resistance | |
| Heat Exchanger Shells | Forming Characteristics | Formability | |
| Heat Exchanger Shells | Mechanical Properties | Moderate Strength | |
| Pump Cylinder Liners | Corrosion Resistance | Corrosion Resistance | |
| Pump Cylinder Liners | Forming Characteristics | Formability | |
| Pump Cylinder Liners | Mechanical Properties | Moderate Strength |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Bar | ASTM | B36/B36M | BRASS PLATE, SHEET, STRIP AND ROLLED BAR | ||
| Plate | ASTM | B36/B36M | BRASS PLATE, SHEET, STRIP AND ROLLED BAR | ||
| Sheet | ASTM | B36/B36M | BRASS PLATE, SHEET, STRIP AND ROLLED BAR | ||
| Strip | ASTM | B36/B36M | BRASS PLATE, SHEET, STRIP AND ROLLED BAR | ||
| Tube | Seamless (Metric) | ASTM | B135/B135M | Seamless Brass Tube | |
| ASTM | B587 | WELDED BRASS TUBE | |||
| ASTM | B135 | Tube, Seamless | |||
| Seamless | ASME | SB135 | SEAMLESS BRASS TUBE |
Corrosion Properties