Find suppliers for this alloyC27200
Chemical Composition
Element
Cu(1)PbZnFe
(1) Cu + Sum of Named Elements 99.7% min.
Min (%)62.0
Max (%)65.00.07Rem0.07
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell F scale
Section Size
(in)
TubeHard DrawnH8074   Typ
55   Typ
10   Typ
80   Typ
0.065
Nominal Grain Size 0.025 mmOS02556   Typ
23   Typ
50   Typ
82   Typ
0.065
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1680
Densitylb/cu in. at 68°F0.305
Specific Gravity8.44
Electrical Conductivity% IACS at 68°F27.6
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F67
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)11.4
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi15000
Modulus of Rigidityksi5600
Fabrication Properties

No fabrication properties for this alloy

Common Fabrication Processes
  • Drawing
  • Forming and Bending
  • Shearing
  • Spinning
  • Swaging
Thermal Characteristics

No thermal characteristics for this alloy

Typical uses
Product Category Product Reason Category Reason
FastenersFastenersCorrosion ResistanceCorrosion Resistance
FastenersForming CharacteristicsFormability
FastenersMechanical PropertiesModerate Strength
IndustrialCold Headed PartsConductivity (Electrical)Electrical Conductivity
Cold Headed PartsConductivity (Thermal)Thermal Conductivity
Cold Headed PartsCorrosion ResistanceCorrosion Resistance
Cold Headed PartsForming CharacteristicsFormability
Heat Exchanger ShellsCorrosion ResistanceCorrosion Resistance
Heat Exchanger ShellsForming CharacteristicsFormability
Heat Exchanger ShellsMechanical PropertiesModerate Strength
Pump Cylinder LinersCorrosion ResistanceCorrosion Resistance
Pump Cylinder LinersForming CharacteristicsFormability
Pump Cylinder LinersMechanical PropertiesModerate Strength
Applicable Specifications
Form Sub-Form Specific Sub-Form System Standard Description
BarASTMB36/B36MBRASS PLATE, SHEET, STRIP AND ROLLED BAR
PlateASTMB36/B36MBRASS PLATE, SHEET, STRIP AND ROLLED BAR
SheetASTMB36/B36MBRASS PLATE, SHEET, STRIP AND ROLLED BAR
StripASTMB36/B36MBRASS PLATE, SHEET, STRIP AND ROLLED BAR
TubeASTMB135Tube, Seamless
Seamless (Metric)ASTMB135MSeamless Brass Tube (Metric)
WeldedASTMB587WELDED BRASS TUBE
Corrosion Properties