| Elements | ||||
|---|---|---|---|---|
| Cu(1) | Pb | Zn | Fe | |
|
(1) Cu + Sum of Named Elements 99.6% min. |
||||
| Min (%) | 65.0 | 0.25 | ||
| Max (%) | 68.0 | 0.7 | Rem | 0.07 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Rockwell F scale | Rockwell 30T scale | Cold Work (%) |
|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||||||
| Tube | Hard | H04 |
75 Typ |
60 Typ |
7 Typ |
80 Typ |
69 Typ |
35 | |
| Nominal Grain Size 0.025 mm | OS025 |
52 Typ |
20 Typ |
50 Typ |
75 Typ |
37 Typ |
|||
| Nominal Grain Size 0.050 mm | OS050 |
47 Typ |
15 Typ |
60 Typ |
64 Typ |
26 Typ |
|||
| Melting Point - Liquidus°F | 1720 |
|---|---|
| Melting Point - Solidus°F | 1660 |
| Densitylb/cu in. at 68°F | 0.307 |
| Specific Gravity | 8.5 |
| Electrical Conductivity% IACS at 68°F | 26 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 67 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 11.2 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 15000 |
| Modulus of Rigidityksi | 5600 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Good |
| Oxyacetylene Welding | Fair |
| Gas Shielded Arc Welding | Fair |
| Coated Metal Arc Welding | Not Recommended |
| Spot Weld | Fair |
| Seam Weld | Not Recommended |
| Butt Weld | Fair |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Poor |
| Machinability Rating | 60 |
Common Fabrication Processes
- Forming and Bending
- Machining
- Piercing and Punching
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 800 | 1200 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Industrial | Power and Pump Cylinder Liners | Corrosion Resistance | Corrosion Resistance |
| Power and Pump Cylinder Liners | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Power and Pump Cylinder Liners | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Power and Pump Cylinder Liners | Machining Characteristics | Machinability | |
| Power and Pump Cylinder Liners | Mechanical Properties | Ductility | |
| Power and Pump Cylinder Liners | Solderability | Solderability | |
| Power and Pump Cylinder Liners | Welding Characteristics | Weldability | |
| Power and Pump Cylinders | Brazing Characteristics | Brazability | |
| Power and Pump Cylinders | Corrosion Resistance | Corrosion Resistance | |
| Power and Pump Cylinders | Finishing Characteristics | Polishable | |
| Power and Pump Cylinders | Machining Characteristics | Machinability | |
| Power and Pump Cylinders | Mechanical Properties | Ductility | |
| Power and Pump Cylinders | Solderability | Solderability | |
| Ordnance | Primers | Corrosion Resistance | Corrosion Resistance |
| Primers | Forming Characteristics | Formability | |
| Primers | Machining Characteristics | Machinability | |
| Primers | Mechanical Properties | Ductility | |
| Primers | Mechanical Properties | Moderate Strength | |
| Plumbing | J Bends | Corrosion Resistance | Corrosion Resistance |
| J Bends | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| J Bends | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| J Bends | Forming Characteristics | Formability | |
| J Bends | Machining Characteristics | Machinability | |
| J Bends | Solderability | Solderability | |
| Plumbing Accessories | Corrosion Resistance | Corrosion Resistance | |
| Plumbing Accessories | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Plumbing Accessories | Forming Characteristics | Formability | |
| Plumbing Accessories | Machining Characteristics | Machinability | |
| Plumbing Accessories | Solderability | Solderability | |
| Plumbing Brass Goods | Corrosion Resistance | Corrosion Resistance | |
| Plumbing Brass Goods | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Plumbing Brass Goods | Forming Characteristics | Formability | |
| Plumbing Brass Goods | Machining Characteristics | Machinability | |
| Plumbing Brass Goods | Solderability | Solderability | |
| Pump Lines | Corrosion Resistance | Corrosion Resistance | |
| Pump Lines | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Pump Lines | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Pump Lines | Forming Characteristics | Formability | |
| Pump Lines | Machining Properties | Machinability, Good | |
| Pump Lines | Solderability | Solderability | |
| Trap Lines | Corrosion Resistance | Corrosion Resistance | |
| Trap Lines | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Trap Lines | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Trap Lines | Forming Characteristics | Formability | |
| Trap Lines | Machining Properties | Machinability, Good | |
| Trap Lines | Solderability | Solderability |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Seamless Tube | ASME | SB135 | SEAMLESS BRASS TUBE | ||
| Tube | FEDERAL | WW-T-791 | TUBING: BRASS, SEAMLESS | ||
| SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |||
| AMS | 4555 | BRASS TUBING SEAMLESS, LIGHT ANNEALED | |||
| MILITARY | MIL-T-46072 | TUBE, ROUND COPPER ALLOYS (LEADED BRASS), SEAMLESS | |||
| Seamless (Metric) | ASTM | B135/B135M | Seamless Brass Tube | ||
| AMS | 4554 | BRASS TUBING, SEAMLESS, LIGHT ANNEALED | |||
| ASTM | B135 | Tube, Seamless | |||
| SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS |
Corrosion Properties